A composite material for virus storage tube and preparation method thereof
By using composite materials with embedded polycondensation chains in virus storage tubes, the problem of polypropylene's adsorption of DNA/RNA is solved, long-term storage without affecting the detection concentration of virus samples is achieved, and the strength and weather resistance of the material are improved.
Patent Information
- Application Number
- CN202310144956.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-21
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2043-02-21
AI Technical Summary
Polypropylene materials have an adsorption effect on DNA/RNA, which causes the detection concentration of virus samples to decrease during storage, affecting the accuracy of detection results.
A composite material is used, including bisphenol A, diphenyl carbonate, polycondensation reaction catalyst, 1-adamantyltrimethylammonium chloride, 2,4,6-triphenylpyranium tetrafluoroborate, 2-Hydroxypropyltrimethylisooctanoic acid ammonium salt , 2-methoxy-5-nitroaniline salt and trimethylstannylmethyldiphenylsilane, a polycarbonate material formed through transesterification reaction and polycondensation reaction, embedded in the polycondensation chain, reducing the impact on DNA and RNA adsorption.
This material does not adsorb DNA and RNA, maintains the detection concentration of virus samples, improves the accuracy of detection results, and has high strength, toughness, acid resistance, alkali resistance and UV resistance, making it suitable for long-term storage of virus samples.
Smart Images

Figure BDA0004088862360000071 
Figure BDA0004088862360000081 
Figure BDA0004088862360000082
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of virus sampling tubes, and more specifically, to a composite material for virus storage tubes and a preparation method thereof. Background Art
[0002] Virus sampling tubes can be used for the collection, transportation and storage of virus samples such as influenza, avian influenza, and coronavirus for subsequent extraction and amplification.
[0003] After the virus samples are collected, PCR testing cannot usually be performed in time at the sample collection site, so the collected virus swab samples need to be transported. The virus itself will quickly break down in vitro, thus affecting subsequent testing. Therefore, virus preservation fluid must be added during storage and transportation. Different virus preservation fluids need to be used for different testing purposes.
[0004] Some virus preservation solutions can lyse and inactivate the virus in the sample, making the virus lose its infectious activity, effectively preventing the operator from secondary infection, and these virus preservation solutions also contain inhibitors that can protect the viral nucleic acid from being degraded, so that subsequent detection by NT-PCR can be performed. In addition, the virus preservation solution can be stored at room temperature for a relatively long time, saving the cost of virus sample storage and transportation.
[0005] The material of current virus storage tubes is generally polypropylene, which has a certain adsorption effect on nucleic acids. When using polypropylene storage tubes to store DNA / RNA, it is easy to cause the DNA / RNA detection concentration to decrease, thereby affecting the accuracy of the test results. Summary of the invention
[0006] In order to improve the problem that the current virus preservation tubes made of polypropylene have a certain adsorption effect on nucleic acids, and the use of polypropylene preservation tubes in the process of storing DNA / RNA easily causes a decrease in DNA / RNA detection concentration, thereby affecting the accuracy of the detection results, the present application proposes a composite material for virus preservation tubes and a preparation method thereof to improve this situation.
[0007] In a first aspect, the present application proposes a composite material for a virus storage tube and adopts the following technical solution.
[0008] A composite material for a virus storage tube. Raw materials for preparing the composite material include bisphenol A, diphenyl carbonate, a polycondensation reaction catalyst, 1-adamantyl trimethyl ammonium chloride, 2,4,6-triphenyl pyrylium tetrafluoroborate, 2-hydroxypropyl trimethyl isooctanoic acid ammonium salt, 2-methoxy-5-nitroaniline hydrochloride and trimethylstannyl methyl diphenyl silane.
[0009] By adopting the above technical scheme, the composite material is suitable for preparing virus preservation tubes, which can be loaded with virus preservation solution and sample for a long time without deterioration. Among them, bisphenol A and diphenyl carbonate generate polycarbonate under the catalysis of polycondensation reaction catalyst, and in the polycondensation process, 1-adamantyl trimethyl ammonium chloride, 2,4,6-triphenyl pyrylium tetrafluoroborate, 2-hydroxypropyl trimethyl isooctanoic acid ammonium salt, 2-methoxy-5-nitroaniline hydrochloride and trimethyl stannyl methyl diphenyl silane are all embedded in the polycondensation chain to modify the polycarbonate. The adamantyl group of 1-adamantyl trimethyl ammonium chloride can improve the strength of the material, and in combination with 2,4,6-triphenyl pyrylium tetrafluoroborate, it can significantly improve the acid resistance, alkali resistance and ultraviolet light resistance of the material. 2-Hydroxypropyltrimethylisooctanoic acid ammonium salt has a multi-branched spatial structure, and 2-methoxy-5-nitroaniline hydrochloride has a spatial strong electron-attracting group. The combination of the two and the polycarbonate chain can significantly reduce the attraction of polycarbonate to DNA and RNA chains, making the material almost non-adsorbing DNA and RNA chains. Trimethylstannylmethyldiphenylsilane has silane and stannyl groups, which can significantly improve the toughness and drop resistance of the material. The combination with 1-adamantyltrimethylammonium chloride also improves the heat resistance and frost resistance of the material. The interaction of the above materials makes the material non-reactive with the virus preservation solution, which is convenient for long-term storage.
[0010] As an improvement of the composite material for virus storage tubes, the raw materials for preparing the composite material include, by mass, 50 to 60 parts of bisphenol A, 50 to 60 parts of diphenyl carbonate, 1 to 3 parts of polycondensation reaction catalysts, 4 to 8 parts of 1-adamantyltrimethylammonium chloride, 5 to 9 parts of 2,4,6-triphenylpyrylium tetrafluoroborate, 6 to 10 parts of 2-hydroxypropyltrimethylisooctanoic acid ammonium salt, 6 to 10 parts of 2-methoxy-5-nitroaniline hydrochloride and 4 to 6 parts of trimethylstannylmethyldiphenylsilane.
[0011] By adopting the above technical scheme, the raw materials are mixed in appropriate proportions, and the prepared composite material has good anti-adsorption properties of DNA and RNA, does not react with virus preservation fluid, has high toughness and is not easy to crack, and is resistant to strong acids and strong alkalis.
[0012] As an improvement of the composite material for virus storage tubes, the raw materials for preparing the composite material include, by mass, 50 parts of bisphenol A, 55 parts of diphenyl carbonate, 2 parts of condensation reaction catalyst, 6 parts of 1-adamantyltrimethylammonium chloride, 7 parts of 2,4,6-triphenylpyrylium tetrafluoroborate, 8 parts of 2-hydroxypropyltrimethylisooctanoic acid ammonium salt, 8 parts of 2-methoxy-5-nitroaniline hydrochloride and 5 parts of trimethylstannylmethyldiphenylsilane.
[0013] By adopting the above technical solution, various properties of the composite material reach an optimal state within a certain test range.
[0014] As an improvement of the composite material for virus storage tube, the polycondensation reaction catalyst includes sodium tetraphenylborate and calcium hydrogen phosphate.
[0015] By adopting the above technical scheme, sodium tetraphenylborate and calcium hydrogen phosphate catalyze the exchange condensation reaction of bisphenol A and diphenyl carbonate, so that the polycondensation reaction can be carried out efficiently and stably.
[0016] As an improvement of the composite material for virus storage tube, the polycondensation reaction catalyst includes 1 part of sodium tetraphenylborate and 1 part of calcium hydrogen phosphate by mass.
[0017] By adopting the above technical scheme, the catalytic efficiency of 1 part of sodium tetraphenylborate and 1 part of calcium hydrogen phosphate is high and the catalyst utilization rate is high.
[0018] As an improvement of the composite material for virus storage tube, the raw materials for preparing the composite material also include cephalaenopsis alkali.
[0019] By adopting the above technical solution, celastrin can further improve the bending strength of the composite material.
[0020] As an improvement of the composite material for virus storage tube, the raw materials for preparing the composite material also include 1 to 3 parts of cephalaenopsis alkaloids.
[0021] By adopting the above technical solution and adding 1 to 3 parts of celastrine, the bending strength of the material can be improved better.
[0022] As an improvement of the composite material for virus storage tube, the raw materials for preparing the composite material also include 1H-pyrrolo[3,2-H]quinoline.
[0023] By adopting the above technical solution, 1H-pyrrolo[3,2-H]quinoline can improve the tensile strength of the composite material.
[0024] As an improvement of the composite material for virus storage tube, the raw materials for preparing the composite material also include 1 to 3 parts of 1H-pyrrolo[3,2-H]quinoline.
[0025] By adopting the above technical solution, adding 1 to 3 parts of 1H-pyrrolo[3,2-H]quinoline to the composite material has the best effect on improving the tensile strength of the material.
[0026] In a second aspect, the present application also proposes a method for preparing a composite material for a virus storage tube, and adopts the following technical solution.
[0027] A method for preparing a composite material for a virus storage tube, the method comprising:
[0028] Bisphenol A, diphenyl carbonate, a polycondensation reaction catalyst, 1-adamantyl trimethyl ammonium chloride, 2,4,6-triphenyl pyrylium tetrafluoroborate, 2-hydroxypropyl trimethyl isooctanoic acid ammonium salt, 2-methoxy-5-nitroaniline hydrochloride and trimethyl stannyl methyl diphenyl silane are added into a reaction kettle, and an ester exchange reaction is carried out at 165-220° C. for 4-8 hours under a pressure of 1-6 kPa, and then the materials are transferred to a polycondensation kettle for a polycondensation reaction at 250-300° C. and a pressure of less than 0.1 kPa for 6-10 hours to obtain the composite material.
[0029] By adopting the above technical scheme, an ester exchange reaction is first carried out to pre-combine the components and fully embed them with each other, and then a condensation reaction is carried out to combine the materials to obtain a composite material with uniform and stable properties.
[0030] In summary, the composite material for virus preservation tubes and the preparation method thereof of the present application have the following beneficial effects: the prepared composite material does not adsorb DNA and RNA, the composite material does not react with the virus preservation solution, and does not affect the detection of DNA and RNA concentrations after virus sampling.
[0031] The prepared composite material has high strength and elastic modulus, high impact strength and a wide operating temperature range.
[0032] The prepared composite material has low molding shrinkage and good dimensional stability.
[0033] The prepared composite material has good weather resistance.
[0034] The prepared composite material is tasteless and odorless, harmless to human body and meets the requirements of sanitation and safety. DETAILED DESCRIPTION
[0035] The following is a detailed description of some embodiments of the composite material for virus storage tube and its preparation method of the present application.
[0036] Example 1
[0037] By mass, 55 parts of bisphenol A, 55 parts of diphenyl carbonate, 1 part of sodium tetraphenylborate, 1 part of calcium hydrogen phosphate, 4 parts of 1-adamantyl trimethyl ammonium chloride, 9 parts of 2,4,6-triphenyl pyrylium tetrafluoroborate, 6 parts of 2-hydroxypropyl trimethyl isooctanoic acid ammonium salt, 10 parts of 2-methoxy-5-nitroaniline hydrochloride and 4 parts of trimethyl stannyl methyl diphenyl silane were added into a reaction kettle, and an ester exchange reaction was carried out at 220° C. for 8 hours under a pressure of 1 kPa, and then the materials were moved to a polycondensation kettle for a polycondensation reaction at 250° C. and a pressure of 50 Pa for 6 hours to obtain the composite material.
[0038] Example 2
[0039] By mass, 60 parts of bisphenol A, 50 parts of diphenyl carbonate, 1 part of sodium tetraphenylborate, 1 part of calcium hydrogen phosphate, 8 parts of 1-adamantyl trimethyl ammonium chloride, 5 parts of 2,4,6-triphenyl pyrylium tetrafluoroborate, 10 parts of 2-hydroxypropyl trimethyl isooctanoic acid ammonium salt, 6 parts of 2-methoxy-5-nitroaniline hydrochloride and 6 parts of trimethyl stannyl methyl diphenyl silane were added into a reaction kettle, and an ester exchange reaction was carried out at 165° C. for 4 hours under a pressure of 6 kPa, and then the materials were moved to a polycondensation kettle for a polycondensation reaction at 300° C. and a pressure of 80 Pa for 10 hours to obtain the composite material.
[0040] Example 3
[0041] By mass, 50 parts of bisphenol A, 55 parts of diphenyl carbonate, 1 part of sodium tetraphenylborate, 1 part of calcium hydrogen phosphate, 6 parts of 1-adamantyl trimethyl ammonium chloride, 7 parts of 2,4,6-triphenyl pyrylium tetrafluoroborate, 8 parts of 2-hydroxypropyl trimethyl isooctanoic acid ammonium salt, 8 parts of 2-methoxy-5-nitroaniline hydrochloride and 5 parts of trimethylstannyl methyl diphenyl silane were added into a reaction kettle, and an ester exchange reaction was carried out at 200° C. for 6 hours under a pressure of 3 kPa, and then the materials were moved to a polycondensation kettle for a polycondensation reaction at 280° C. and a pressure of 30 Pa for 8 hours to obtain the composite material.
[0042] Example 4
[0043] This embodiment adopts a scheme that is substantially the same as that of Embodiment 3, the only difference being that one portion of cephalaenopsis alkaloids is further added to the raw materials of this embodiment.
[0044] By mass, 50 parts of bisphenol A, 55 parts of diphenyl carbonate, 1 part of sodium tetraphenylborate, 1 part of calcium hydrogen phosphate, 6 parts of 1-adamantyl trimethyl ammonium chloride, 7 parts of 2,4,6-triphenyl pyrylium tetrafluoroborate, 8 parts of 2-hydroxypropyl trimethyl isooctanoic acid ammonium salt, 8 parts of 2-methoxy-5-nitroaniline hydrochloride, 5 parts of trimethyl stannyl methyl diphenyl silane and 1 part of cephaladine were added into a reaction kettle, and an ester exchange reaction was carried out at 200° C. under a pressure of 3 kPa for 6 hours, and then the materials were moved to a polycondensation kettle for a polycondensation reaction at 280° C. and a pressure of 30 Pa for 8 hours to obtain the composite material.
[0045] Example 5
[0046] This embodiment adopts a scheme that is substantially the same as that of Embodiment 3, the only difference being that 3 portions of cephalaenopsis linalool are further added to the raw materials of this embodiment.
[0047] By mass, 50 parts of bisphenol A, 55 parts of diphenyl carbonate, 1 part of sodium tetraphenylborate, 1 part of calcium hydrogen phosphate, 6 parts of 1-adamantyl trimethyl ammonium chloride, 7 parts of 2,4,6-triphenyl pyrylium tetrafluoroborate, 8 parts of 2-hydroxypropyl trimethyl isooctanoic acid ammonium salt, 8 parts of 2-methoxy-5-nitroaniline hydrochloride, 5 parts of trimethyl stannyl methyl diphenyl silane and 3 parts of leucoderma serrata were added into a reactor, and an ester exchange reaction was carried out at 200° C. under a pressure of 3 kPa for 6 hours, and then the materials were moved to a polycondensation kettle for a polycondensation reaction at 280° C. and a pressure of 30 Pa for 8 hours to obtain the composite material.
[0048] Example 6
[0049] This example adopts a scheme that is substantially the same as that of Example 3, with the only difference being that one portion of 1H-pyrrolo[3,2-H]quinoline is further added to the raw materials of this example.
[0050] By mass, 50 parts of bisphenol A, 55 parts of diphenyl carbonate, 1 part of sodium tetraphenylborate, 1 part of calcium hydrogen phosphate, 6 parts of 1-adamantyl trimethyl ammonium chloride, 7 parts of 2,4,6-triphenyl pyrylium tetrafluoroborate, 8 parts of 2-hydroxypropyl trimethyl isooctanoic acid ammonium salt, 8 parts of 2-methoxy-5-nitroaniline hydrochloride, 5 parts of trimethyl stannyl methyl diphenyl silane and 1 part of 1H-pyrrolo[3,2-H]quinoline were added into a reaction kettle, and an ester exchange reaction was carried out at 200° C. under a pressure of 3 kPa for 6 hours, and then the materials were moved to a polycondensation kettle for a polycondensation reaction at 280° C. and a pressure of 30 Pa for 8 hours to obtain the composite material.
[0051] Example 7
[0052] This example adopts a scheme that is substantially the same as that of Example 3, the only difference being that 3 portions of 1H-pyrrolo[3,2-H]quinoline are further added to the raw materials of this example.
[0053] By mass, 50 parts of bisphenol A, 55 parts of diphenyl carbonate, 1 part of sodium tetraphenylborate, 1 part of calcium hydrogen phosphate, 6 parts of 1-adamantyl trimethyl ammonium chloride, 7 parts of 2,4,6-triphenyl pyrylium tetrafluoroborate, 8 parts of 2-hydroxypropyl trimethyl isooctanoic acid ammonium salt, 8 parts of 2-methoxy-5-nitroaniline hydrochloride, 5 parts of trimethyl stannyl methyl diphenyl silane and 3 parts of 1H-pyrrolo[3,2-H]quinoline were added into a reaction kettle, and an ester exchange reaction was carried out at 200° C. under a pressure of 3 kPa for 6 hours, and then the materials were moved to a polycondensation kettle for a polycondensation reaction at 280° C. and a pressure of 30 Pa for 8 hours to obtain the composite material.
[0054] Example 8
[0055] This example adopts a scheme that is substantially the same as that of Example 3, with the only difference being that 2 parts of cephalaenopsis linalool and 2 parts of 1H-pyrrolo[3,2-H]quinoline are further added to the raw materials of this example.
[0056] By mass, 50 parts of bisphenol A, 55 parts of diphenyl carbonate, 1 part of sodium tetraphenylborate, 1 part of calcium hydrogen phosphate, 6 parts of 1-adamantyl trimethyl ammonium chloride, 7 parts of 2,4,6-triphenylpyrylium tetrafluoroborate, 8 parts of 2-hydroxypropyl trimethyl isooctanoic acid ammonium salt, 8 parts of 2-methoxy-5-nitroaniline hydrochloride, 5 parts of trimethylstannylmethyl diphenylsilane, 2 parts of leucophylline and 2 parts of 1H-pyrrolo[3,2-H]quinoline were added into a reaction kettle, and an ester exchange reaction was carried out at 200° C. under a pressure of 3 kPa for 6 hours, and then the materials were moved to a polycondensation kettle for a polycondensation reaction at 280° C. and a pressure of 30 Pa for 8 hours to obtain the composite material.
[0057] Comparative Example 1
[0058] This comparative example adopts a scheme that is substantially the same as that of Example 3, with the only difference being that the raw material 1-adamantyltrimethylammonium chloride is not added in this comparative example. The details of this scheme are as follows.
[0059] By mass, 50 parts of bisphenol A, 55 parts of diphenyl carbonate, 1 part of sodium tetraphenylborate, 1 part of calcium hydrogen phosphate, 7 parts of 2,4,6-triphenylpyrylium tetrafluoroborate, 8 parts of 2-hydroxypropyltrimethylisooctanoic acid ammonium salt, 8 parts of 2-methoxy-5-nitroaniline hydrochloride and 5 parts of trimethylstannylmethyldiphenylsilane were added into a reaction kettle, and an ester exchange reaction was carried out at 200° C. for 6 hours under a pressure of 3 kPa. The materials were then transferred to a polycondensation kettle for a polycondensation reaction at 280° C. and a pressure of 30 Pa for 8 hours to obtain the composite material.
[0060] Comparative Example 2
[0061] This comparative example adopts a scheme that is substantially the same as that of Example 3, the only difference being that the raw material 2,4,6-triphenylpyrylium tetrafluoroborate is not added in this comparative example. The details of this scheme are as follows.
[0062] By mass, 50 parts of bisphenol A, 55 parts of diphenyl carbonate, 1 part of sodium tetraphenylborate, 1 part of calcium hydrogen phosphate, 6 parts of 1-adamantyl trimethyl ammonium chloride, 8 parts of 2-hydroxypropyl trimethyl isooctanoic acid ammonium salt, 8 parts of 2-methoxy-5-nitroaniline hydrochloride and 5 parts of trimethylstannyl methyl diphenyl silane were added into a reaction kettle, and an ester exchange reaction was carried out at 200° C. under a pressure of 3 kPa for 6 hours. The materials were then transferred to a polycondensation kettle for a polycondensation reaction at 280° C. and a pressure of 30 Pa for 8 hours to obtain the composite material.
[0063] Comparative Example 3
[0064] This comparative example adopts a scheme that is basically the same as Example 3, the only difference being that the raw material 2-hydroxypropyltrimethylisooctanoic acid ammonium salt is not added in this comparative example. The details of this scheme are as follows.
[0065] By mass, 50 parts of bisphenol A, 55 parts of diphenyl carbonate, 1 part of sodium tetraphenylborate, 1 part of calcium hydrogen phosphate, 6 parts of 1-adamantyl trimethyl ammonium chloride, 7 parts of 2,4,6-triphenyl pyrylium tetrafluoroborate, 8 parts of 2-methoxy-5-nitroaniline hydrochloride and 5 parts of trimethylstannyl methyl diphenyl silane were added into a reaction kettle, and an ester exchange reaction was carried out at 200° C. for 6 hours under a pressure of 3 kPa. The materials were then transferred to a polycondensation kettle for a polycondensation reaction at 280° C. and a pressure of 30 Pa for 8 hours to obtain the composite material.
[0066] Comparative Example 4
[0067] This comparative example adopts a scheme that is substantially the same as that of Example 3, the only difference being that the raw material 2-methoxy-5-nitroaniline hydrochloride is not added in this comparative example. The details of this scheme are as follows.
[0068] By mass, 50 parts of bisphenol A, 55 parts of diphenyl carbonate, 1 part of sodium tetraphenylborate, 1 part of calcium hydrogen phosphate, 6 parts of 1-adamantyl trimethyl ammonium chloride, 7 parts of 2,4,6-triphenyl pyrylium tetrafluoroborate, 8 parts of 2-hydroxypropyl trimethyl isooctanoic acid ammonium salt and 5 parts of trimethyl stannyl methyl diphenyl silane were added into a reaction kettle, and an ester exchange reaction was carried out at 200° C. for 6 hours under a pressure of 3 kPa. The materials were then transferred to a polycondensation kettle for a polycondensation reaction at 280° C. and a pressure of 30 Pa for 8 hours to obtain the composite material.
[0069] Comparative Example 5
[0070] This comparative example adopts a scheme that is basically the same as Example 3, the only difference being that the raw material trimethylstannylmethyldiphenylsilane is not added in this comparative example. The details of this scheme are as follows.
[0071] By mass, 50 parts of bisphenol A, 55 parts of diphenyl carbonate, 1 part of sodium tetraphenylborate, 1 part of calcium hydrogen phosphate, 6 parts of 1-adamantyl trimethyl ammonium chloride, 7 parts of 2,4,6-triphenyl pyrylium tetrafluoroborate, 8 parts of 2-hydroxypropyl trimethyl isooctanoic acid ammonium salt and 8 parts of 2-methoxy-5-nitroaniline hydrochloride were added into a reaction kettle, and an ester exchange reaction was carried out at 200° C. for 6 hours under a pressure of 3 kPa, and then the materials were moved to a polycondensation kettle for a polycondensation reaction at 280° C. and a pressure of 30 Pa for 8 hours to obtain the composite material.
[0072] Test Example 1
[0073] The composite materials prepared in Examples 1 to 8 and Comparative Examples 1 to 5 were all made into virus storage tubes, and the following corresponding tests were carried out.
[0074] The same inactivated viral RNA solution was loaded into the virus storage tubes and polypropylene tubes prepared from the composite materials of Examples 1 to 8 and Comparative Examples 1 to 5 and allowed to stand for 4 hours, and then the RNA solution in each virus storage tube was poured out to detect its RNA concentration. Among them, the RNA concentration of the inactivated viral RNA solution was 30 ng / μL. The RNA concentration results of each tube after standing for 4 hours are shown in Table 1 below.
[0075] Table 1 Comparative test of RNA adsorption by various materials
[0076]
[0077]
[0078] As can be seen from Table 1, the composite materials prepared in Examples 1 to 8 do not basically adsorb RNA, which shows that they have almost no effect on the detection of the sampled viral RNA concentration. The materials prepared in Comparative Examples 1, 2, and 5 were used to load viral RNA, and the tested RNA concentration decreased slightly. It can be seen that the materials in these three comparative examples have a slight adsorption effect on RNA. The materials prepared in Comparative Examples 3 and 4 were loaded with viral RNA, and the tested RNA concentration decreased by 3ng / μL. The material in Comparative Example 3 did not add 2-hydroxypropyltrimethylisooctanoic acid ammonium salt, and the material prepared in Comparative Example 4 did not add 2-methoxy-5-nitroaniline hydrochloride. It can be seen that the combination of the two has the effect of reducing the attraction of the composite material to the RNA chain. The use of polypropylene tubes to load viral RNA liquid reduced the RNA detection concentration by 4ng / μL. It can be seen that polypropylene has a certain adsorption effect on nucleic acids. The use of polypropylene storage tubes in the process of storing DNA / RNA is likely to cause the DNA / RNA detection concentration to decrease, thereby affecting the accuracy of the test results.
[0079] Test Example 2
[0080] The composite materials prepared in Examples 1 to 8 and Comparative Examples 1 to 5 were all made into plates, and the following corresponding tests were carried out, as shown in Table 2.
[0081] Table 2 Physical properties test of composite materials prepared in various embodiments and comparative examples
[0082]
[0083]
[0084] As can be seen from Table 2, the composite materials prepared in Examples 1 to 8 have good tensile strength, tensile elongation at break, flexural strength and Rockwell hardness. Compared with Example 1, Examples 4 and 5 further add the raw material cephalosporin, and the flexural strength of the material is improved to a certain extent. Compared with Example 1, Examples 6 and 7 further add the raw material 1H-pyrrolo[3,2-H]quinoline, which improves the tensile strength of the composite material. Compared with Example 1, Example 8 adds the raw materials cephalosporin and 1H-pyrrolo[3,2-H]quinoline, and the flexural strength and tensile strength of the material are improved to a certain extent.
[0085] Compared with Example 1, Comparative Example 1, in which the raw material 1-adamantyltrimethylammonium chloride was not added, has a significant decrease in tensile strength, tensile elongation at break, flexural strength and Rockwell hardness. It can be seen that the addition of 1-adamantyltrimethylammonium chloride improves the strength of the material.
[0086] Compared with Example 1, Comparative Example 2 does not add the raw material 2,4,6-triphenylpyrylium tetrafluoroborate, and its tensile strength, tensile elongation at break, flexural strength and Rockwell hardness all decrease slightly. It can be seen that the addition of 2,4,6-triphenylpyrylium tetrafluoroborate is also helpful in improving the strength of the material.
[0087] Compared with Example 1, Comparative Example 3 does not add the raw material 2-hydroxypropyltrimethylisooctanoic acid ammonium salt, and its material strength remains basically unchanged.
[0088] Compared with Example 1, Comparative Example 4 does not add the raw material 2-methoxy-5-nitroaniline hydrochloride, and its material strength remains basically unchanged.
[0089] Compared with Example 1, in Comparative Example 5, the raw material trimethylstannylmethyldiphenylsilane was not added, and its tensile elongation at break and flexural strength were significantly reduced. It can be seen that the addition of trimethylstannylmethyldiphenylsilane has a great effect on improving the toughness of the composite material.
[0090] Test Example 3
[0091] The composite materials prepared in Examples 1 to 8 and Comparative Examples 1 to 5 were all made into plates, and the following corresponding tests were carried out, as shown in Table 3.
[0092] Table 3 Comparison of physical and chemical test results of composite materials prepared in various embodiments and comparative examples
[0093]
[0094] It can be seen from Table 3 that the composite materials prepared in Examples 1 to 8 have good acid resistance, alkali resistance, UV resistance, and high and low temperature resistance.
[0095] The composite material prepared in Comparative Example 1 does not contain 1-adamantyltrimethylammonium chloride, and its acid resistance, alkali resistance and UV resistance are all reduced, and its high and low temperature resistance is also reduced.
[0096] The composite material prepared in Comparative Example 2 does not contain 2,4,6-triphenylpyrylium tetrafluoroborate, and its acid resistance, alkali resistance and UV resistance are all reduced.
[0097] The composite material prepared in Comparative Example 3 did not contain 2-hydroxypropyltrimethylisooctanoate ammonium salt, and its acid resistance and high temperature resistance were reduced.
[0098] The composite material prepared in Comparative Example 4 did not contain 2-methoxy-5-nitroaniline hydrochloride, and its acid resistance and low temperature resistance were both reduced.
[0099] The composite material prepared in Comparative Example 5 does not contain trimethylstannylmethyldiphenylsilane, and its high and low temperature resistance performance is significantly reduced.
[0100] In summary, the common raw materials of Examples 1 to 8, 1-adamantyl trimethyl ammonium chloride, 2,4,6-triphenyl pyrylium tetrafluoroborate, 2-hydroxypropyl trimethyl isooctanoic acid ammonium salt, 2-methoxy-5-nitroaniline hydrochloride and 2-methoxy-5-nitroaniline hydrochloride, have a great effect on the physical and chemical properties of the composite material. The various raw materials cooperate with each other and the polycarbonate chains are interlocked with each other to jointly improve the strength, toughness, acid and alkali resistance, UV resistance, high and low temperature resistance and other properties of the composite material. The lack of any raw material will cause a significant decrease in material performance.
[0101] The composite materials prepared in Examples 1 to 8 do not adsorb DNA and RNA, do not react with the virus preservation solution, and do not affect the detection of DNA and RNA concentrations after virus sampling. The composite materials have high strength and elastic modulus, high impact strength, and a wide operating temperature range. The composite materials are tasteless and odorless, harmless to the human body, and meet health and safety requirements.
[0102] The above is only a preferred embodiment of the present application, and the protection scope of the present application is not limited to the above embodiment. All technical solutions under the concept of the present application belong to the protection scope of the present application. It should be pointed out that for ordinary technicians in this technical field, some improvements and modifications without departing from the principle of the present application should also be regarded as falling within the protection scope of the present application.
Claims
1. A composite material for a virus storage tube, characterized in that: The raw materials for preparing the composite material include, by mass, 50 to 60 parts of bisphenol A, 50 to 60 parts of diphenyl carbonate, 1 to 3 parts of a polycondensation reaction catalyst, 4 to 8 parts of 1-adamantyl trimethyl ammonium chloride, 5 to 9 parts of 2,4,6-triphenyl pyrylium tetrafluoroborate, 6 to 10 parts of 2-hydroxypropyl trimethyl isooctanoic acid ammonium salt, 6 to 10 parts of 2-methoxy-5-nitroaniline hydrochloride and 4 to 6 parts of trimethylstannyl methyl diphenyl silane; The preparation method of the composite material comprises: adding bisphenol A, diphenyl carbonate, a polycondensation reaction catalyst, 1-adamantyl trimethyl ammonium chloride, 2,4,6-triphenyl pyrylium tetrafluoroborate, 2-hydroxypropyl trimethyl isooctanoic acid ammonium salt, 2-methoxy-5-nitroaniline hydrochloride and trimethyl stannyl methyl diphenyl silane into a reaction kettle, carrying out an ester exchange reaction at 165-220° C. for 4-8 hours under a pressure of 1-6 kPa, and then transferring the materials to a polycondensation kettle for a polycondensation reaction at 250-300° C. and a pressure of less than 0.1 kPa for 6-10 hours to obtain the composite material.
2. The composite material for virus storage tube according to claim 1, characterized in that: The raw materials for preparing the composite material include, by mass, 50 parts of bisphenol A, 55 parts of diphenyl carbonate, 2 parts of polycondensation catalyst, 6 parts of 1-adamantyltrimethylammonium chloride, 7 parts of 2,4,6-triphenylpyrylium tetrafluoroborate, 8 parts of 2-hydroxypropyltrimethylisooctanoic acid ammonium salt, 8 parts of 2-methoxy-5-nitroaniline hydrochloride and 5 parts of trimethylstannylmethyldiphenylsilane.
3. The composite material for virus storage tube according to claim 1 or 2, characterized in that: The polycondensation reaction catalyst includes sodium tetraphenylborate and calcium hydrogen phosphate.
4. The composite material for virus storage tube according to claim 3, characterized in that: The polycondensation reaction catalyst includes 1 part of sodium tetraphenylborate and 1 part of calcium hydrogen phosphate by mass.
5. The composite material for virus storage tube according to claim 1, characterized in that: The raw materials for preparing the composite material also include cephalaenopsis alkali.
6. The composite material for virus storage tube according to claim 5, characterized in that: The raw materials for preparing the composite material also include 1 to 3 parts of cephalaenopsis alkaloids by mass.
7. The composite material for virus storage tube according to claim 1, characterized in that: The raw materials for preparing the composite material also include 1H-pyrrolo[3,2-H]quinoline.
8. The composite material for virus storage tube according to claim 7, characterized in that: The raw materials for preparing the composite material further include 1 to 3 parts of 1H-pyrrolo[3,2-H]quinoline by mass.
9. A method for preparing a composite material for a virus storage tube according to any one of claims 1 to 8, characterized in that: The preparation method comprises: Bisphenol A, diphenyl carbonate, a polycondensation reaction catalyst, 1-adamantyl trimethyl ammonium chloride, 2,4,6-triphenyl pyrylium tetrafluoroborate, 2-hydroxypropyl trimethyl isooctanoic acid ammonium salt, 2-methoxy-5-nitroaniline hydrochloride, trimethyl stannyl methyl diphenyl silane, optional cephaladine and optional 1H-pyrrolo[3,2-H]quinoline are added into a reaction kettle, and an ester exchange reaction is carried out at 165-220° C. for 4-8 hours under a pressure of 1-6 kPa, and then the materials are transferred to a polycondensation kettle for a polycondensation reaction at 250-300° C. and a pressure of less than 0.1 kPa for 6-10 hours to obtain the composite material.
Citation Information
Patent Citations
Preparation process of polycarbonate
CN106947072A
Polycarbonate nanocomposites
US20120149839A1