A conductive hydrogel biointerface material and its preparation method and application

By introducing N-hydroxysuccinimide into the hydrogel, grafting polyacrylic polymer and other components, the conductive hydrogel biointerface material is formed, which solves the low conductivity of existing hydrogels in the field of bioelectronics. The problems of increased mechanical modulus and poor stability have achieved high toughness bonding and high conductivity biointerface materials, suitable for biomedical electronic devices and in vivo electrical stimulation treatment.

CN116178867BActive Publication Date: 2024-12-03SOUTHERN UNIVERSITY OF SCIENCE AND TECHNOLOGY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211581728.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-09
Publication Date
2024-12-03
Estimated Expiration
2042-12-09

AI Technical Summary

Technical Problem

The application of existing hydrogel materials in the field of bioelectronics is due to the problems of low conductivity, increased mechanical modulus, high preparation cost and poor stability adhesion, and it is difficult to take into account both electrical, mechanical, biological compatibility and stability. Adhesion ability.

Method used

Using N-hydroxysuccinimide grafted polyacrylic acid polymers, conductive polymers, polyvinyl alcohols and polyamino polymers, the conductive hydrogel biointerface material is formed through uniform mixing and cross-linking to ensure that it is in Rapid drainage, chemical bonding and high toughness bonding on biological tissues improve conductivity and electrochemical properties.

Benefits of technology

It has achieved high toughness bonding and conductivity of more than 9S/m, and has excellent stability and biocompatibility. It is suitable for the preparation of biomedical electronic devices and in vivo electrical stimulation treatment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116178867B_ABST
    Figure CN116178867B_ABST
Patent Text Reader

Abstract

The present invention discloses a conductive hydrogel biointerface material and its preparation method and application, the method comprising the steps of: uniformly mixing a polyacrylic acid polymer solution grafted with N-hydroxysuccinimide and a conductive polymer to obtain a first mixed solution; uniformly mixing a polyvinyl alcohol solution, a polyamino polymer solution and a crosslinking agent solution to obtain a second mixed solution; mixing the first mixed solution with the second mixed solution to obtain a hydrogel precursor solution; processing the hydrogel precursor solution to the surface of a substrate, and obtaining a conductive hydrogel biointerface material after curing. The present invention introduces N-hydroxysuccinimide group polymers in the preparation of the hydrogel, so that the hydrogel can quickly drain water at the wet interface and promote chemical bonding between the hydrogel and biological tissues; introducing amino polymers and polyvinyl alcohol to form a stable crosslinking network inside the hydrogel to ensure the formation of high-toughness hydrogel bioadhesion; introducing a conductive polymer to give the bioadhesive high conductivity and electrochemical properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of biomedical materials, and in particular to a conductive hydrogel biointerface material and a preparation method and application thereof. Background Art

[0002] The progress of modern electronic technology has led to the rapid development of medical detection and treatment equipment, which can provide patients with personalized physiological information detection, and can also play an important role in the diagnosis and treatment of certain diseases, making a huge contribution to human health. Compared with traditional medical devices, bioelectronic devices are in closer contact with biological tissues and are directly fixed on the surface or inside of target tissues and organs. They can more realistically detect the physiological state of tissues / organs and carry out targeted treatment in a timely manner. However, human organs and modern electrical appliances have completely different and even contradictory properties in terms of materials. Biological tissues are soft, high-water content active substances, while electronic devices are rigid, water-free, inactive substances, which seriously affects the interaction and fusion between the two.

[0003] Recent studies have found that hydrogels have mechanical properties similar to those of biological tissues and high water content, which are extremely similar to biological tissues. They are considered to be one of the ideal interface materials for building a perfect fusion of human-machine interfaces. However, compared with biological tissues, existing hydrogel materials still have some functional deficiencies. For example, most of the current hydrogels are ion conductive, and the conductivity is generally lower than 1S / m, which seriously limits their further application in the field of bioelectronics. In order to solve this problem, researchers usually add conductive nanoparticles (such as gold nanoparticles, carbon nanotubes and graphene, etc.) into the preparation of hydrogels to improve the electrical conductivity of hydrogels. However, the large difference between the size and spatial arrangement of conductive nanoparticles and polymer chains is filled into the hydrogel through physical interaction, which may cause the mechanical modulus of the hydrogel to increase, and produce adverse mechanical interactions when in contact with the cell membrane, which may produce potential cytotoxicity; in addition, the introduction of materials such as precious metals may cause a substantial increase in the cost of hydrogel preparation, which is not conducive to the development of hydrogel bioelectronics. In addition, for hydrogel interface materials, it is not only required to conduct electrical interaction between electrodes and biological tissues, but also to be able to stably fix electronic devices on the surface of target tissues. However, due to the presence of surface moisture, most current hydrogel materials are difficult to form stable and firm adhesion with various interfaces (such as electronic devices, engineering materials, human tissues, etc.), and it is difficult to perform long-term stable work. The above-mentioned deficiencies limit the development of hydrogels into biological interface materials.

[0004] Therefore, the prior art still needs to be improved and developed. Summary of the invention

[0005] In view of the above-mentioned deficiencies in the prior art, the purpose of the present invention is to provide a conductive hydrogel biointerface material and a preparation method and application thereof, aiming to solve the problem that it is difficult for existing hydrogels to simultaneously take into account the electrical, mechanical, biocompatibility and stable adhesion ability with target tissues to meet the needs of practical applications.

[0006] The technical solution of the present invention is as follows:

[0007] A conductive hydrogel biointerface material, wherein the conductive hydrogel biointerface material comprises a polyacrylic acid polymer solution grafted with N-hydroxysuccinimide, a conductive polymer, a polyvinyl alcohol solution, a polyamino polymer solution and a crosslinking agent solution.

[0008] The conductive hydrogel biointerface material, wherein the mass percentage of the polyvinyl alcohol solution is 2-20%, the mass percentage of the polyamino polymer solution is 1-10%, and the mass percentage of the crosslinking agent solution is 0.01-0.1%.

[0009] A method for preparing a conductive hydrogel biointerface material, comprising the steps of:

[0010] Providing N-hydroxysuccinimide grafted polyacrylic acid polymer solution;

[0011] Evenly mixing the N-hydroxysuccinimide grafted polyacrylic acid polymer solution and the conductive polymer to obtain a first mixed solution;

[0012] Mixing the polyvinyl alcohol solution, the polyamino polymer solution and the crosslinking agent solution uniformly to obtain a second mixed solution;

[0013] Evenly mixing the first mixed solution and the second mixed solution to obtain a hydrogel precursor solution;

[0014] The hydrogel precursor solution is processed onto the surface of a substrate and solidified to obtain a conductive hydrogel biointerface material.

[0015] The method for preparing the conductive hydrogel biointerface material, wherein the step of preparing the N-hydroxysuccinimide grafted polyacrylic acid polymer solution comprises:

[0016] Adding acrylic acid and acrylic acid N-hydroxysuccinimide to an anhydrous dimethyl sulfoxide solution, then adding an azo initiator, stirring evenly and heating to react, to obtain a reaction solution;

[0017] After the reaction solution is cooled to room temperature, the reaction solution is slowly added dropwise to an acetone solution to precipitate a milky white polymer, which is then transferred to a clean beaker and placed in a vacuum drying oven for drying to obtain a polyacrylic acid polymer grafted with N-hydroxysuccinimide;

[0018] The N-hydroxysuccinimide grafted polyacrylic acid polymer is dissolved in deionized water to prepare an N-hydroxysuccinimide grafted polyacrylic acid polymer solution.

[0019] The method for preparing the conductive hydrogel biointerface material, wherein the mass ratio of the acrylic acid to the acrylic acid N-hydroxysuccinimide ester is 2-30:1.

[0020] The method for preparing the conductive hydrogel biointerface material, wherein the temperature of the heating reaction is 50-90° C. and the time is 2-48 hours.

[0021] The method for preparing the conductive hydrogel biointerface material, wherein in the first mixed solution, the conductive polymer accounts for 1-20% of the total weight.

[0022] The method for preparing the conductive hydrogel biointerface material comprises the following steps: the mass percentage of the polyvinyl alcohol solution is 2-20%, the mass percentage of the polyamino polymer solution is 1-10%, and the mass percentage of the crosslinking agent solution is 0.01-0.1%.

[0023] The method for preparing the conductive hydrogel biointerface material, wherein, in the hydrogel precursor solution, the volume ratio of the first mixed solution to the second mixed solution is 1:0.2-5.

[0024] The method for preparing the conductive hydrogel biointerface material, wherein the substrate comprises a metal electrode, a carbon electrode, polyethylene, polyurethane, PET, PI, PC and PDMS.

[0025] A conductive hydrogel biointerface material is prepared by the method for preparing the conductive hydrogel biointerface material of the present invention.

[0026] An application of a conductive hydrogel biointerface material, wherein the conductive hydrogel biointerface material prepared by the preparation method of the invention is used to prepare biomedical electronic devices.

[0027] Beneficial effects: The present invention introduces N-hydroxysuccinimide group polymers in the preparation of hydrogels, so that the hydrogels can quickly drain water at the wet interface and chemically bond between the hydrogels and biological tissues; introduces amino polymers and polyvinyl alcohol to form a stable cross-linked network inside the hydrogel to ensure the formation of high-toughness hydrogel bioadhesion; introduces conductive polymers to give the bioadhesive high conductivity and electrochemical properties. Therefore, the present invention creatively develops a conductive hydrogel biointerface material with adhesion properties. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 The present invention is a flow chart of a method for preparing a conductive hydrogel biointerface material.

[0029] Figure 2 This is a graph showing the adhesion performance results between the conductive hydrogel biointerface material provided by the present invention and biological tissue.

[0030] Figure 3 This is a graph showing the adhesion performance results of the conductive hydrogel interface material provided by the present invention and different substrates.

[0031] Figure 4 This is a graph showing the conductivity stability results of the conductive bioadhesive provided by the present invention in a liquid environment. DETAILED DESCRIPTION

[0032] The present invention provides a conductive hydrogel biointerface material and a preparation method and application thereof. To make the purpose, technical solution and effect of the present invention clearer and more specific, the present invention is further described in detail below. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0033] See also Figure 1 , Figure 1 The present invention provides a flow chart of a method for preparing a conductive hydrogel biointerface material, as shown in the figure, which comprises the following steps:

[0034] S10, providing a polyacrylic acid polymer solution grafted with N-hydroxysuccinimide;

[0035] S20, uniformly mixing the N-hydroxysuccinimide grafted polyacrylic acid polymer solution and the conductive polymer to obtain a first mixed solution;

[0036] S30, mixing the polyvinyl alcohol solution, the polyamino polymer solution and the cross-linking agent solution uniformly to obtain a second mixed solution;

[0037] S40, uniformly mixing the first mixed solution and the second mixed solution to obtain a hydrogel precursor solution;

[0038] S50, processing the hydrogel precursor liquid onto the surface of the substrate, and obtaining a conductive hydrogel biointerface material after curing.

[0039] Specifically, in order to simultaneously ensure the adhesion, electrical and electrochemical properties of the conductive hydrogel biointerface material, the present invention selects N-hydroxysuccinimide grafted polyacrylic acid polymer as the A component for preparing the hydrogel, which can effectively promote the hydrogel to quickly absorb moisture on the interface of moist biological tissues and play a role in drainage; and the N-hydroxysuccinimide group reacts rapidly with the amino group on the biological tissue to form a covalent crosslink to form a strong and tough biological interface adhesion; the present invention also selects a class of polyamino polymers as the B component for preparing the hydrogel. After blending, the N-hydroxysuccinimide group can quickly form a crosslinking network with amino-containing polymers such as chitosan to ensure the formation of a high-toughness hydrogel; a class of conductive polymers is selected as the C component for preparing the hydrogel, which can give the hydrogel good electrical properties and provide a good electrical interaction platform for electronic devices and biological tissues; polyvinyl alcohol is selected as the D component for preparing the hydrogel, which can ensure the toughness of the hydrogel; a class of dialdehyde structure compounds is selected as the E component for preparing the hydrogel as the crosslinking agent of the system. By adjusting the proportion of each component, the optimal formula for preparing conductive hydrogel biointerface materials with adhesion properties can be obtained.

[0040] The conductive hydrogel biointerface material with adhesive properties provided by the present invention can form high-toughness adhesion with various biological tissues and engineering materials, which is superior to the current commercial bioadhesives; in addition, the interface material has a high electrical conductivity, and its conductivity is greater than 9Sm -1 , which is superior to most ion-conductive hydrogels and has excellent stability in physiological environments. After being immersed in PBS buffer solution for more than two weeks, its conductivity remains stable. The conductive hydrogel biointerface material with adhesion properties provided by the present invention can be developed and applied to the preparation of electronic equipment for monitoring physiological signals in organisms (such as monitoring electrocardiogram signals, electromyography signals and electroencephalogram signals), as well as in vivo electrical stimulation treatment equipment, etc.

[0041] In some embodiments, the steps of preparing a polyacrylic acid polymer solution grafted with N-hydroxysuccinimide include: adding acrylic acid and acrylic acid N-hydroxysuccinimide ester to an anhydrous dimethyl sulfoxide solution, then adding an azo initiator, stirring evenly and heating to react to obtain a reaction solution; after the reaction solution is cooled to room temperature, slowly dropping the reaction solution into an acetone solution to precipitate a milky white polymer, transferring it to a clean beaker, and placing it in a vacuum drying oven to dry to obtain a polyacrylic acid polymer grafted with N-hydroxysuccinimide; dissolving the polyacrylic acid polymer grafted with N-hydroxysuccinimide in deionized water to obtain a polyacrylic acid polymer solution grafted with N-hydroxysuccinimide. In this embodiment, the polyacrylic acid polymer grafted with N-hydroxysuccinimide is obtained by copolymerization of acrylic acid and acrylic acid N-hydroxysuccinimide ester, and its structural formula is as follows: Wherein, x and y are independently selected from numbers between 0 and 1, and the sum of x and y is 1. As an example, x can be 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8 or 0.9, etc., and y can be 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8 or 0.9, etc., but are not limited to the values ​​listed above, and other values ​​not listed in the above numerical range are also applicable. Preferably, in the polyacrylic acid polymer grafted with N-hydroxysuccinimide, when x is 0.6-0.9 and y is 0.1-0.4, the prepared hydrogel has better adhesion properties.

[0042] In this embodiment, the mass ratio of acrylic acid to N-hydroxysuccinimide acrylate is 2-30:1. For example, the mass ratio of acrylic acid to N-hydroxysuccinimide acrylate can be 30:1, 20:1, 10:1, 5:1, 2:1, etc.

[0043] In the process of preparing the N-hydroxysuccinimide grafted polyacrylic acid polymer solution in this embodiment, the heating reaction temperature is 50-90°C and the time is 2-48h; after the reaction, the temperature of drying in a vacuum drying oven is 20-50°C.

[0044] In this embodiment, N-hydroxysuccinimide grafted polyacrylic acid polymer is selected as component A for preparing the hydrogel, which can effectively promote the hydrogel to quickly absorb moisture on the interface of wet biological tissues and play a role in drainage. In addition, the N-hydroxysuccinimide group reacts quickly with the amino group on the biological tissue to form covalent crosslinks, thereby forming a strong biological interface adhesion.

[0045] In some embodiments, in the first mixed solution, the conductive polymer accounts for 1-20% of the total weight. In this embodiment, the conductive polymer is selected as the C component for preparing the hydrogel, which can give the hydrogel good electrical properties and provide a good electrical interaction platform for electronic devices and biological tissues. In this embodiment, the conductive polymer is one or more of polyaniline, polypyrrole, polyfuran and polyindole poly(3,4-ethylenedioxythiophene): poly(styrene sulfonate), but is not limited thereto.

[0046] In some embodiments, the mass percentage of the polyvinyl alcohol solution is 2-20%, the mass percentage of the polyamino polymer solution is 1-10%, and the mass percentage of the crosslinking agent solution is 0.01-0.1%. In this embodiment, the polyamino polymer can be one or more of chitosan, carboxymethyl chitosan, carboxyethyl chitosan, gelatin and amino-polyethylene glycol-amino, but is not limited thereto, wherein the deacetylation degree of the chitosan is 80-90%, and the molecular weight of the amino-polyethylene glycol-amino is 1,000-100,000Da. In this embodiment, the molecular weight of the polyvinyl alcohol is 1,000-300,000Da, preferably 100,000-300,000Da. In this embodiment, the cross-linking agent is a compound with a dialdehyde structure at the terminal group, such as one of glyoxal, malondialdehyde, succindialdehyde, glutaraldehyde, adipaldehyde, and aldehyde-polyethylene glycol-aldehyde (CHO-PEG-CHO), wherein the molecular weight of the aldehyde-polyethylene glycol-aldehyde is 100-2,000Da, preferably 100-600Da.

[0047] In some embodiments, during the preparation of the hydrogel precursor solution, the volume ratio of the first mixed solution to the second mixed solution is 1:0.2-5. For example, the volume ratio of the first mixed solution to the second mixed solution is 1:0.2; 1:0.5; 1:0.8; 1:1; 1:1.2; 1:1.5; 1:2; 1:3; 1:5, etc., but is not limited to the above-listed values, and other values ​​not listed in the above numerical range are also applicable.

[0048] In some embodiments, the viscosity of the hydrogel precursor prepared by the present invention is highly adjustable, so it can be prepared on different substrate surfaces through various processing methods, and the hydrogel precursor formula can be adjusted according to the specific application scenario; various substrates coated with hydrogel are placed under different conditions for curing to obtain conductive hydrogel biointerface materials with adhesion properties. Among them, the processing method includes: one of spin coating, drip coating, dip coating, scraping, injection, printing and printing; the substrate includes metal electrodes, carbon electrodes, polyethylene, polyurethane, PET, PI, PC and PDMS; the curing method is drying in a closed, air or nitrogen environment for 3-48 hours.

[0049] In some embodiments, a conductive hydrogel biointerface material is also provided, the conductive hydrogel biointerface material comprising a polyacrylic acid polymer solution grafted with N-hydroxysuccinimide, a conductive polymer, a polyvinyl alcohol solution, a polyamino polymer solution, and a crosslinking agent solution. In this embodiment, the mass percentage of the polyvinyl alcohol solution is 2-20%, the mass percentage of the polyamino polymer solution is 1-10%, and the mass percentage of the crosslinking agent solution is 0.01-0.1%.

[0050] In some embodiments, an application of a conductive hydrogel biointerface material is also provided, wherein the conductive hydrogel biointerface material prepared by the preparation method of the present invention is used to prepare a biomedical electronic device. In this embodiment, the biomedical electronic device includes an electronic device for monitoring electrocardiogram signals, electromyogram signals and electroencephalogram signals, as well as an in vivo electrical stimulation treatment device, etc.

[0051] The present invention will be further explained below by means of specific embodiments:

[0052] Example 1

[0053] This embodiment provides a conductive hydrogel interface material with adhesion properties, and its components and proportions are as follows:

[0054] Solution A:

[0055] Components Dosage(g) PAA-NHS 0.2 Conductive polymers 0.05 Deionized water 1

[0056] Solution B:

[0057] Components Dosage(g) PVA 0.1 Chitosan 0.02 Glutaraldehyde 0.0001 water 1

[0058] The preparation method is as follows: PAA-NHS and conductive polymer are dissolved and dispersed in 1g of water, mixed and defoamed to obtain solution A; PVA, chitosan and glutaraldehyde are dissolved in 1g of water, mixed and defoamed to obtain solution B; A and B are mixed and defoamed, and injected into the mold, and then the solvent is evaporated and vacuum dried to obtain a conductive hydrogel biointerface material.

[0059] Example 2

[0060] This embodiment provides a conductive hydrogel interface material with adhesion properties, and its components and proportions are as follows:

[0061] Solution A:

[0062] Components Dosage(g) PAA-NHS 0.25 Conductive polymers 0.03 Deionized water 1

[0063] Solution B:

[0064] Components Dosage(g) PVA 0.12 gelatin 0.05 CHO-PEG-CHO (mw~200) 0.0005 water 1

[0065] The preparation method is as follows: PAA-NHS and conductive polymer are dissolved and dispersed in 1 g of water, mixed and defoamed to obtain solution A; PVA, gelatin, and CHO-PEG-CHO are dissolved in 1 g of water, mixed and defoamed to obtain solution B; A and B are mixed and defoamed, and printed on a PET substrate, and then the solvent is evaporated and dried in the air to obtain a conductive hydrogel biointerface material.

[0066] Example 3

[0067] This embodiment provides a conductive hydrogel interface material with adhesion properties, and its components and proportions are as follows:

[0068] Solution A:

[0069] Components Dosage(g) PAA-NHS 0.3 Conductive polymers 0.06 Deionized water 1

[0070] Solution B:

[0071] Components Dosage(g) PVA 0.08 Chitosan 0.03 CHO-PEG-CHO (mw~600) 0.001 water 1

[0072] The preparation method is as follows: PAA-NHS and conductive polymer are dissolved and dispersed in 1g of water, mixed and defoamed to obtain solution A; PVA, chitosan, and CHO-PEG-CHO are dissolved in 1g of water, mixed and defoamed to obtain solution B; A and B are mixed and defoamed, and printed onto a PDMS substrate, and then the solvent is evaporated and dried in the air to obtain a conductive hydrogel biointerface material.

[0073] Example 4

[0074] This embodiment provides a conductive hydrogel interface material with adhesion properties, and its components and proportions are as follows:

[0075] Solution A:

[0076]

[0077]

[0078] Solution B:

[0079] Components Dosage(g) PVA 0.13 Chitosan 0.01 CHO-PEG-CHO (mw~100) 0.0002 water 1

[0080] The preparation method is as follows: PAA-NHS and conductive polymer are dissolved and dispersed in 1 g of water, mixed and defoamed to obtain solution A; PVA, chitosan, and CHO-PEG-CHO are dissolved in 1 g of water, mixed and defoamed to obtain solution B; A and B are mixed and defoamed, and then dip-coated on a platinum electrode, and then the solvent is evaporated and dried in air to obtain a conductive hydrogel biointerface material.

[0081] Test Case

[0082] Characterization of the interfacial adhesion properties of conductive hydrogel biointerface materials and different biological tissues. Figure 2As shown. First, attach the prepared conductive hydrogel interface adhesive material to the surface of the biological tissue, press the hydrogel gently, the polyacrylic acid inside the hydrogel will quickly absorb moisture from the tissue surface, the polymer molecular chain will fully contact the tissue, and then NHS will form a chemical cross-linking effect with the amino group on the tissue surface, thereby forming a high-toughness bond. Then use strong glue (such as: 502, etc.) to apply to the other side of the hydrogel bio-interface material, and bond the non-deformable nylon backing to this side. Pay attention to the use of glue during the operation to prevent the glue from infiltrating into the bonding interface with the biological tissue. The adhesion performance of the hydrogel bio-interface material and the biological tissue was evaluated by two methods: 180° peel test and shear strength test. The corresponding test results are shown in Figure 2 As shown, the results indicate that the biointerface material can form high-toughness adhesion with various biological tissues (such as heart, skin, blood vessels, etc.).

[0083] Characterization of the interfacial adhesion properties of conductive hydrogel biointerface materials and different solid substrate materials. Figure 3 As shown. First, various substrates are surface cleaned and activated, and the substrate materials (PET, PI, PDMS or Au-PET) are respectively immersed in ethanol and acetone solutions, each ultrasonic treatment lasts for 5-15 minutes, repeated three times, and dried under nitrogen conditions to obtain a cleaned electrode substrate; the surface of the cleaned electrode substrate is oxygen plasma cleaned and activated for 5-30 minutes to obtain an activated electrode substrate, at which time the substrate surface will have a large number of hydroxyl groups. The treated substrate is immersed in a 0.1-0.5% solution of 3-aminopropyltriethoxysilane. 3-aminopropyltriethoxysilane will hydrolyze in a water environment, and the ethoxy group will first hydrolyze into a hydroxyl group, and then react with the hydroxyl group on the surface of the substrate, dehydrate to form a Si-O-Si bond, and the three ethoxy groups of 3-aminopropyltriethoxysilane react into hydroxyl groups, resulting in the hydrolysis products being easily condensed with each other, thereby forming a polysiloxane molecular modification layer with amino groups on the surface of the above-mentioned substrate. Then, PBS solution was sprayed on the modified substrate surface, and then the conductive hydrogel biointerface material was bonded to various substrate surfaces. Since the reaction mechanism was consistent with the previous article, the NHS groups inside the hydrogel would chemically crosslink with the amino groups on the substrate surface, thereby forming a high-toughness bond. The 180° peel test and shear strength test were also used to evaluate the interfacial bonding strength between the hydrogel and the substrate. The results are shown in Figure 2. Figure 3 shown.

[0084] The test results of the conductivity stability of conductive hydrogel biointerface materials are as follows: Figure 4The prepared hydrogel material was immersed in PBS buffer solution. After swelling equilibrium, the resistance of the hydrogel sample was tested with two probes, and then the conductivity of the hydrogel was calculated. The stability of the hydrogel in the solution was tested. The test results showed that the hydrogel was able to remain stable for up to two weeks, and the conductivity was always maintained at 9Sm. -1 above.

[0085] It should be understood that the application of the present invention is not limited to the above examples. For ordinary technicians in this field, improvements or changes can be made based on the above description. All these improvements and changes should fall within the scope of protection of the claims attached to the present invention.

Claims

1. A method for preparing a conductive hydrogel biointerface material, characterized in that: Includes steps: Providing N-hydroxysuccinimide grafted polyacrylic acid polymer solution; Evenly mixing the N-hydroxysuccinimide grafted polyacrylic acid polymer solution and the conductive polymer to obtain a first mixed solution; Adding polyvinyl alcohol, polyamino polymer and cross-linking agent into water and mixing evenly to obtain a second mixed solution; Evenly mixing the first mixed solution and the second mixed solution to obtain a hydrogel precursor solution; The hydrogel precursor solution is processed onto the surface of a substrate and solidified to obtain a conductive hydrogel biointerface material.

2. The method for preparing the conductive hydrogel biointerface material according to claim 1, characterized in that: The step of providing a polyacrylic acid polymer solution grafted with N-hydroxysuccinimide comprises: Mixing acrylic acid and acrylic acid N-hydroxysuccinimide ester, adding the mixture into an anhydrous dimethyl sulfoxide solution, and then adding an azo initiator, stirring the mixture evenly, and heating the mixture to react, thereby obtaining a reaction solution; After the reaction solution is cooled to room temperature, the reaction solution is slowly added dropwise to an acetone solution to precipitate a milky white polymer, which is then placed in a vacuum drying oven for drying to obtain a polyacrylic acid polymer grafted with N-hydroxysuccinimide; The N-hydroxysuccinimide grafted polyacrylic acid polymer is dissolved in deionized water to prepare an N-hydroxysuccinimide grafted polyacrylic acid polymer solution.

3. The method for preparing the conductive hydrogel biointerface material according to claim 2, characterized in that: The mass ratio of the acrylic acid to the acrylic acid N-hydroxysuccinimide ester is 2-30:

1.

4. The method for preparing the conductive hydrogel biointerface material according to claim 2, characterized in that: The temperature of the heating reaction is 50-90° C. and the time is 2-48 hours.

5. The method for preparing the conductive hydrogel biointerface material according to claim 1, characterized in that: In the first mixed solution, the conductive polymer accounts for 1-20% of the total weight.

6. The method for preparing the conductive hydrogel biointerface material according to claim 1, characterized in that: The substrate is one of a metal electrode, a carbon electrode, polyethylene, polyurethane, PET, PI, PC and PDMS.

7. A conductive hydrogel biointerface material, characterized in that: The conductive hydrogel biointerface material is prepared by the preparation method of any one of claims 1 to 6.

8. An application of a conductive hydrogel biointerface material, characterized in that: The conductive hydrogel biointerface material according to claim 7 is used to prepare biomedical electronic devices.