A kind of degradable courier bag material and preparation method thereof

By using 2,2-bis(P-aminophenoxy)ethyl ether and 4,4'-diaminodibenzocrown ether, a prepolymer with a "rigid and flexible" structure is formed, and combined with low density polyethylene and Camellia peel powder solves the problem of poor compatibility of degradable plastics in the existing technology and realizes high-performance degradable express bag materials with excellent mechanical properties and environmental friendliness.

CN116178887BActive Publication Date: 2024-10-29DONGHUA UNIV +2
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202310121211.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-16
Publication Date
2024-10-29
Estimated Expiration
2043-02-16

AI Technical Summary

Technical Problem

Existing degradable plastic products have poor compatibility between fillers and polymers, resulting in cracks and holes on the surface, affecting their toughness and tensile strength. They cannot simultaneously meet the degradability and impact and tear resistance of express bags. Performance requirements.

Method used

Using 2,2-bis(P-aminophenoxy)ethyl ether and 4,4'-diaminodibenzocrown ether as monomers, a prepolymer with a "rigid and soft" structure is formed through polycondensation reaction. The low-density polyethylene and camellia peel powder in the filler masterbatch are used to prepare composite materials with cyclic and non-cyclic structures, which improve thermal degradation stability and tensile strength, and achieve complete degradation through microbial degradation.

Benefits of technology

It has achieved higher thermal degradation stability, tensile strength and resistance to organic solvents. The material is easily degraded in inorganic acid liquid, its mechanical properties are better than national standards, and its cost is low, making it more competitive in the market.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004079988990000011
    Figure HDA0004079988990000011
  • Figure HDA0004079988990000021
    Figure HDA0004079988990000021
  • Figure HDA0004079988990000022
    Figure HDA0004079988990000022
Patent Text Reader

Abstract

The invention discloses a degradable courier bag material and a preparation method thereof, and belongs to the technical field of degradable polymer materials. The specific courier bag material comprises the following components calculated by weight: 20-40 parts of 2,2-bis(P-aminophenoxy)ethyl ether, 5-15 parts of 4,4'-diaminodibenzocrown ether, 25-45 parts of paraformaldehyde (PFA), 10-20 parts of N-methylpyrrolidone, 2-5 parts of polycaprolactone, 5-15 parts of filler masterbatch, and 0.5-1.5 parts of lubricant. The degradable courier bag prepared by using this component comprehensively utilizes the characteristics of different natural degradable materials and different resin raw materials. It also contains cyclic and non-cyclic aromatic diamines with flexible ethylene diether and rigid benzene ring structure characteristics, namely 4,4'-diaminodibenzocrown ether and 2,2-bis(P-aminophenoxy) ether. The two are reacted with polyformaldehyde to prepare a new type of PHT resin, and then the filler masterbatch is prefabricated to make it have good mechanical properties and degradation properties at the same time, and the manufacturing process is simple. Compared with traditional courier bags, under the condition of the same cost, the degradability is significantly increased, and it is a resource-saving and environmentally friendly product.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of degradable polymer materials, and in particular to a degradable express bag material and a preparation method and application thereof. Background Art

[0002] With the update and upgrade of people's lifestyles, consumption concepts and payment methods, online shopping is no longer the main venue for young people in cities. Driven by the popularization of smart phones and new social e-commerce, the online market in China has fully penetrated into rural towns and villages. This has also become a new growth point and a battleground for the e-commerce industry. People of all ages can enjoy the convenience brought by technology, and the elderly can also easily buy their favorite products online.

[0003] More than 300 million tons of plastic products are produced worldwide each year, most of which are discarded within a year. The non-degradability of these materials and the generation of toxic gases during incineration require environmentally friendly new degradable materials to achieve green resources through advanced solid waste management methods. Developed countries such as Europe, the United States, and Japan have begun to adopt local bans and mandatory pollution fees to reduce pollution for plastic products that are non-degradable or difficult to degrade in nature. However, this type of degradable plastic filler has poor compatibility with polymers, and there are cracks and holes on the surface, which will affect the toughness and tensile strength of plastic products. The patent 202010372818.1 "A polyethylene-based degradable plastic and its preparation method" is composed of polyethylene, starch, a degrading agent, a degradation promoter, a modifier, a plasticizer and a lubricant, an antioxidant and titanium dioxide, and the mechanical properties cannot meet the requirements of national standard express packaging bags. The existing technology cannot simultaneously meet the requirements of express bags with good degradability and mechanical properties such as impact resistance and tear resistance. Summary of the invention

[0004] In view of the above problems existing in the prior art, the object of the present invention is to provide a degradable express bag material and a preparation method and application thereof.

[0005] In order to achieve the above-mentioned invention object, the technical solution adopted by the present invention is as follows:

[0006] A degradable courier bag material, characterized in that it comprises the following components calculated by weight: 20-40 parts of 2,2-bis(P-aminophenoxy)ethyl ether, 5-15 parts of 4,4'-diaminodibenzocrown ether, 25-45 parts of paraformaldehyde (PFA), 10-20 parts of N-methylpyrrolidone, 2-5 parts of polycaprolactone, 5-15 parts of filler masterbatch, and 0.5-1.5 parts of lubricant;

[0007] The filler masterbatch includes the following components calculated by weight: 10-25 parts of calcium carbonate, 5-20 parts of talcum powder, 10-20 parts of camellia peel powder, and 10-20 parts of low-density polyethylene.

[0008] As a preferred embodiment, the mass fraction of 2,2-bis(P-aminophenoxy)ethyl ether is 90%-98%.

[0009] As a preferred solution, the mass fraction of the 4,4'-diaminodibenzocrown ether is 90%-98%.

[0010] As a preferred embodiment, the lubricant is one or more of stearic acid, stearate, oleamide, palmitic acid, and ethylene bisstearamide.

[0011] As a preferred embodiment, the compatibilizer is glycidyl methacrylate.

[0012] As a preferred solution, the mass fraction of the paraformaldehyde is 92%-95%.

[0013] The present invention also provides a method for preparing the above-mentioned degradable courier bag material, comprising the following steps:

[0014] S1, taking a certain amount of paraformaldehyde and adding it to a mixed solvent of NMP and water (water content is 12-15 vol%), and heating the mixture to 80-85° C. to depolymerize the paraformaldehyde into a clear formaldehyde liquid;

[0015] S2, cool the clarified liquid and transfer it to a 45-55°C oil bath to maintain constant temperature;

[0016] S3, adding 5 mol% of 2,2-bis(P-aminophenoxy)ethyl ether or 4,4'-diaminodibenzocrown ether monomer to the formaldehyde solution, stirring and reacting at 45-55° C. for 10-15 minutes to prepare a prepolymer mixture;

[0017] S4, pouring the prepolymer mixture into a mold made of tetrafluoroethylene, placing it in a 45-55°C forced air drying oven for 20-30 hours, and then keeping it at 130-150°C for 5-7 hours to remove the solvent as much as possible to obtain a solidified mixture;

[0018] S5. Weigh the calcium carbonate, talcum powder, camellia peel powder and low-density polyethylene in the formula, mix them in a high-speed blender, and extrude and granulate them in an extruder to prepare a filling masterbatch.

[0019] S6. Weigh the mixture, polycaprolactone, filler masterbatch, lubricant, and compatibilizer according to the formula components, put the component materials into a mixer and mix them evenly, put the mixed materials into an extruder at a temperature of 130-160° C., extrude, cool, and granulate;

[0020] S7. Add the particles obtained in step S6 into a film blowing machine, raise the temperature to 150-170°C for film blowing, and add the particles into a bag making machine after cooling to form a degradable express bag material.

[0021] Compared with the prior art, the present invention has the following significant beneficial effects:

[0022] 1. A new type of degradable material containing cyclic and non-cyclic structural units was prepared using two monomers with "rigid and flexible" structural characteristics: 2,2-bis(P-aminophenoxy)ethyl ether and 4,4'-diaminodibenzo crown ether. Preparation process exploration shows that the cyclic and non-cyclic structural units of the two degradable express bag materials affect the formation of HT cross-linked structures, showing higher thermal degradation stability and hydrophilicity. It is easier to degrade in inorganic acid solutions. At the same time, its rigid structural units can give the material better tensile strength, hydrophobicity and better resistance to organic solvents.

[0023] 2. The filler masterbatch uses low-density polyethylene as a carrier and has good compatibility with the matrix resin. The filler masterbatch is evenly dispersed in the composite material, which increases the material gap to a certain extent. Camellia peel powder helps to induce the invasion of microorganisms. After being degraded by microorganisms in the environment, it will cause defects and damage on the surface of the composite material. It helps microorganisms or enzymes to directly interact with polymers in the composite material, decomposing or oxidizing the polymers into small molecules until they are completely degraded to generate carbon dioxide and water. Camellia peel powder has low cost and realizes the recycling of waste resources, making this product more competitive in the sales market. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 It is a synthetic route map of the degradable courier bag material prepared by the present invention;

[0025] Figure 2 is a cross-sectional electron micrograph of the degradable courier bag material prepared by the present invention (Example 1);

[0026] Figure 3 is a cross-sectional electron microscope image of the degradable courier bag material prepared by the present invention (Comparative Example 2);

[0027] Figure 4 These are the performance test results of various embodiments of the degradable courier bag material prepared by the present invention. DETAILED DESCRIPTION

[0028] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0029] The polycondensation reaction of two diamines, 2,2-bis(p-aminophenoxy)ethyl ether and 4,4'-diaminodibenzocrown ether, with formaldehyde is essentially an addition condensation process between amino groups and formaldehyde. Figure 1 As shown in (a) and (b), in the prepolymerization stage of the reaction at 40-60°C, a hemiacetal dynamic covalent adaptive network structure (HDCNs) is formed. At 130-150°C and in the subsequent high-temperature curing process, the solvent NMP is evaporated, and the dynamic covalent network is dehydrated to form a hexahydrotriazine (HT) ring to obtain PHT resin.

[0030] Example 1

[0031] A degradable courier bag, comprising the following components (kg):

[0032] 2,2-bis(P-aminophenoxy)ethyl ether 30, 4,4'-diaminodibenzocrown ether 15, paraformaldehyde (PFA) 30, N-methylpyrrolidone 14, polycaprolactone 5, filler masterbatch 10, lubricant 1.

[0033] The above formula can be used to produce a degradable courier bag. The method for making the degradable courier bag is as follows:

[0034] S1, adding the above-mentioned proportion of paraformaldehyde into a mixed solvent of NMP and water (water content is 12-vol%), and heating the mixture to 80° C. to depolymerize the paraformaldehyde into a clear formaldehyde liquid;

[0035] S2, cool the clarified liquid and transfer it to a 50°C oil bath to maintain constant temperature;

[0036] S3, adding 5 mol % of 2,2-bis(P-aminophenoxy)ethyl ether or 4,4'-diaminodibenzocrown ether monomer to the formaldehyde solution, stirring and reacting at 50° C. for 12 min to prepare a prepolymer mixture;

[0037] S4, pouring the prepolymer mixture into a mold made of tetrafluoroethylene, placing it in a 50° C. forced air drying oven for 24 hours, and then keeping it at 150° C. for 6 hours to remove the solvent as much as possible to obtain a solidified mixture;

[0038] S5, weighing the formula amount of calcium carbonate, talcum powder, camellia peel powder, and low-density polyethylene, mixing them in a high-speed blender, and extruding and granulating them through an extruder to prepare a filling masterbatch;

[0039] S6. Weigh the mixture, polycaprolactone, filler masterbatch, lubricant, and compatibilizer according to the formula components, put the component materials into a mixer and mix them evenly, put the mixed materials into an extruder at a temperature of 150° C., extrude, cool, and granulate;

[0040] S7. Add the particles obtained in step S6 into a film blowing machine, raise the temperature to 160°C for film blowing, and add the particles into a bag making machine after cooling to make a degradable express bag material.

[0041] Example 2

[0042] A degradable courier bag, comprising the following components (kg):

[0043] 2,2-bis(P-aminophenoxy)ethyl ether 20, 4,4'-diaminodibenzo crown ether 15, polyformaldehyde (PFA) 35, N-methylpyrrolidone 14, polycaprolactone 5, filler masterbatch 10, lubricant 1

[0044] The above formula can be used to produce degradable courier bags, and the preparation process is the same as that in Example 1, which will not be repeated here.

[0045] Example 3

[0046] A degradable courier bag, comprising the following components (kg):

[0047] 2,2-bis(P-aminophenoxy)ethyl ether 40, 4,4'-diaminodibenzo crown ether 10, polyformaldehyde (PFA) 25, N-methylpyrrolidone 12, polycaprolactone 2, filler masterbatch 10, lubricant 1

[0048] The above formula can be used to produce degradable courier bags, and the preparation process is the same as that in Example 1, which will not be repeated here.

[0049] Comparative Example 1

[0050] A degradable courier bag, comprising the following components (kg):

[0051] 2,2-bis(P-aminophenoxy)ethyl ether 30, 4,4'-diaminodibenzo crown ether 15, polyformaldehyde (PFA) 30, N-methylpyrrolidone 14, polycaprolactone 5, filler masterbatch 10, lubricant 1

[0052] The above formula can be used to produce degradable express bags. The difference from Example 1 is that during the preparation process, S4 is only placed in a 50°C forced air drying oven for 24 hours. The rest is the same as Example 1 and will not be repeated here.

[0053] Comparative Example 2

[0054] A degradable courier bag, comprising the following components (kg):

[0055] 4,4'-Diaminodibenzocrown ether 45, polyformaldehyde (PFA) 30, N-methylpyrrolidone 14, polycaprolactone 5, filler masterbatch 10, lubricant 1

[0056] The above formula can be used to produce degradable courier bags, and the preparation process is the same as that in Example 1, which will not be repeated here.

[0057] Comparative Example 3

[0058] A degradable courier bag, comprising the following components (kg):

[0059] 2,2-bis(P-aminophenoxy)ethyl ether 45, polyformaldehyde (PFA) 30, N-methylpyrrolidone 14, polycaprolactone 5, filler masterbatch 10, lubricant 1

[0060] The above formula can be used to produce degradable courier bags, and the preparation process is the same as that in Example 1, which will not be repeated here.

[0061] Performance Testing

[0062] The degradable courier bags prepared in the embodiments of the present invention and the comparative examples were subjected to the following performance tests, and the test results are shown in Figure 4 :

[0063] 1. Determination of tensile strength: in accordance with the national standard "Determination of tensile properties of plastics" (GB\T1040.3).

[0064] 2. Determination of elongation at break: in accordance with the national standard "Determination of tensile properties of plastics" (GB / T1040.1).

[0065] 3. Determination of right-angle tear force: in accordance with the national standard "Test method for right-angle tear performance of plastics" (GB\T1130).

[0066] 4. Determination of weight loss rate: Compare the mass of the product before and after 120 days of burial after exposure to light, and calculate the weight loss rate.

[0067] From the above results of Examples 1-3, it can be seen that the weight loss rate of the degradable courier bags prepared by the present invention after 120 days is more than 75%, which is significantly improved compared with traditional courier bags. For example, the tensile strength of the degradable material prepared in Example 1 can reach 36.5MPa, and the right-angle tear force can reach 5.6N. The mechanical properties are better than the performance requirements of the national standard (GB\T16606.3-2018) for express packaging products for courier bags. In addition, it can be seen from Comparative Example 1 that the mechanical properties and degradable properties of the prepared product are reduced when the heat preservation is not performed for h to remove the solvent as much as possible to obtain a solidified mixture.

[0068] In the case of not adding 2,2-bis(P-aminophenoxy)ethyl ether, the material mechanical properties of the comparative example 2 are poor due to the poor compatibility of the composite material, and cannot meet the application requirements of the express bag. Similarly, the weight loss rate of the comparative example 3 is lower than that of the embodiments 1-3, and the effect of the present invention cannot be achieved.

[0069] Finally, it should be pointed out that the above are only some preferred embodiments of the present invention and should not be construed as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made by those skilled in the art based on the above contents of the present invention all fall within the scope of protection of the present invention.

Claims

1. A degradable courier bag material, characterized in that: The invention comprises the following components calculated by weight: 20-40 parts of 2,2-bis(P-aminophenoxy)ethyl ether, 5-15 parts of 4,4'-diaminodibenzo-18-crown ether-6, 25-45 parts of paraformaldehyde (PFA), 10-20 parts of N-methylpyrrolidone, 2-5 parts of polycaprolactone, 5-15 parts of filler masterbatch, 0.5-1.5 parts of lubricant, and also comprises a compatibilizer; The filler masterbatch includes the following components calculated by weight: 10-25 parts of calcium carbonate, 5-20 parts of talc, 10-20 parts of camellia peel powder, and 10-20 parts of low-density polyethylene; And a method for preparing a degradable courier bag material, comprising the following steps: S1, taking a certain amount of paraformaldehyde and adding it to a mixed solvent of NMP and water, wherein the water content is 12-15 vol%, and heating the mixture to 80-85°C to depolymerize the paraformaldehyde into a clear formaldehyde liquid; S2, cool the clarified liquid and transfer it to a 45-55 ℃ oil bath to maintain a constant temperature; S3, adding 5 mol% of 2,2-bis(P-aminophenoxy)ethyl ether and 4,4'-diaminodibenzo-18-crown-6 monomer to the formaldehyde solution, stirring and reacting at 45-55°C for 10-15 min to prepare a prepolymer mixture; S4, pouring the prepolymer mixture into a mold made of tetrafluoroethylene, placing it in a 45-55°C forced air drying oven for 20-30 hours, and then keeping it at 130-150°C for 5-7 hours to remove the solvent as much as possible to obtain a solidified mixture; S5, weighing the calcium carbonate, talcum powder, camellia peel powder, and low-density polyethylene in a formula amount, mixing them in a high-speed blender, and extruding and granulating them in an extruder to prepare a filling masterbatch; S6. Weigh the mixture, polycaprolactone, filler masterbatch, lubricant, and compatibilizer according to the formula components, put the component materials into a mixer and mix them evenly, put the mixed materials into an extruder at a temperature of 130-160° C., extrude, cool, and granulate; S7. Add the particles obtained in step S6 into a film blowing machine, raise the temperature to 150-170°C for film blowing, and add the particles into a bag making machine after cooling to form a degradable express bag material.

2. A degradable courier bag material according to claim 1, characterized in that: The mass fraction of the 2,2-bis(P-aminophenoxy)ethyl ether is 90%-98%.

3. The degradable courier bag material according to claim 1, characterized in that: The mass fraction of the 4,4'-diaminodibenzo-18-crown ether-6 is 90%-98%.

4. The degradable courier bag material according to claim 1, characterized in that: The lubricant is one or more of stearic acid, stearate, oleamide, palmitic acid, and ethylene bisstearamide.

5. The degradable courier bag material according to claim 1, characterized in that: The compatibilizer is glycidyl methacrylate.

6. The degradable courier bag material according to claim 1, characterized in that: The mass fraction of the paraformaldehyde is 92%-95%.

7. Application of the degradable express bag material according to any one of claims 1 to 6 in the express packaging industry.

Citation Information

Patent Citations

  • Polyethylene-based degradable plastic and preparation method thereof

    CN111471233A

  • Formulations comprising cyclic compounds

    CN101541346A

  • Coating solution for forming functional polymer film, and method for forming functional polymer film

    CN103403113A

  • Coating solution for forming polyimide film, liquid crystal alignment agent, polyimide film, liquid crystal alignment film, and liquid crystal display element

    CN103415583A

  • Acid controllable degradation type cycloaliphatic epoxy resin and preparation method thereof