Anti-stick coating for demoulding of refractory prefabricated materials and preparation method thereof
By using anti-stick coatings composed of water glass solution, refractory aggregate, hardener and suspension agent, the complex film formation process, slow curing speed and safety hazards of refractory prefabricated materials are solved, and simplified mold release is achieved The process and efficient sintering effect reduce costs and improve production efficiency.
Patent Information
- Application Number
- CN202211680387.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-26
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2042-12-26
AI Technical Summary
The anti-stick coatings commonly used when refractory prefabricated materials are demolded in molding, with cumbersome film forming process, slow curing speed, high cost, and may burn and smoke at high temperatures, which have safety and environmental protection problems, and cannot effectively solve large or special-shaped prefabricated parts. Demolding problem.
Anti-stick coating composed of water glass solution, refractory aggregate, hardening agent and suspension agent is used. After simple mixing, spray or apply it on the inner wall of the mold to form an anti-stick film of 0.2 to 1mm thickness, and a gap is formed with the mold after hardening. , reduces adhesion, facilitates mold release, and sintered with refractory prefabricated materials during drying to form a whole.
The mold release process is simplified, the curing speed is fast, the cost is low, and the irritating gas is not generated at high temperatures, and it does not remain on the mold, which improves production efficiency and reduces appearance defects.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of coatings, and in particular to an anti-sticking coating for demoulding refractory prefabricated materials and a preparation method thereof. Background Art
[0002] Refractory prefabricated materials refer to a type of refractory material prepared by prefabrication. The process of prefabricated material molding is as follows: the mixed material after adding water and stirring evenly is loaded into the mold, and the material is vibrated and exhausted to form a dense and uniform whole. After a certain period of curing, the required prefabricated material can be obtained by demolding. Affected by factors such as the slurry condition of the mixed material, the surface roughness of the metal mold and the processing accuracy, the mixed material of the prefabricated material is very easy to adhere to the mold, resulting in poor appearance such as roughness, missing edges and corners on the surface of the semi-finished product after demolding. In severe cases, the semi-finished product may be scrapped due to severe damage after demolding.
[0003] The commonly used anti-sticking coatings are: 1. Buy expensive release agents on the market; this release agent has a limited effect on demolding and anti-sticking. It can play a good role in demolding and anti-sticking for small prefabricated parts, but for large and special-shaped prefabricated parts, due to the large contact area between the mixture and the mold and the many corners, this release agent still cannot solve the problem of demolding and anti-sticking. 2. Brush a layer of calcium-based grease, waste oil and other oily materials on the inner surface of the mold; this type of material also has the problem of not being able to solve the problem of demolding and anti-sticking for large and special-shaped prefabricated materials. At the same time, because the production process of refractory prefabricated parts requires that the semi-finished products must undergo a drying process (200-400℃), this type of oily substance will burn and smoke during the drying process, which poses safety and environmental protection problems. In addition, this type of oily substance is liquid or semi-solid. If it is applied too much, it will be adsorbed on the surface of the mixture during the vibration molding process of the mixture, resulting in appearance defects such as pockmarks on the surface of the semi-finished product after drying. If it is applied too little, it will not play an anti-sticking role. 3. Pad paper on the surface of the mold; Pad paper on the surface of the mold can effectively prevent the adhesion between the mold and the mixture, but during the vibration molding process of the mixture, the paper padding on the surface of the mold can easily be rolled into the mixture, resulting in poor product appearance. At the same time, if the rolled paper forms holes after drying, it will cause safety risks in product use.
[0004] In addition, Liu Sheng et al. studied a room-temperature curable solvent-based anti-stick coating for solid rocket propellant demolding in "Research on Room-Temperature Curing Anti-stick Coating" (China Surface Engineering, 2008, (02), 31-35). Although the coating can form a coating under room temperature conditions, the entire coating film drying process takes 10 days, which is too long to be used in industrial production.
[0005] For example, the Chinese patent application document with publication number CN110951396A discloses an anti-stick coating, which requires high-temperature sintering treatment of the release agent surface with flame (treatment temperature is 1200-2200°C). This method involves hot work, which has safety hazards in industrial production and is not conducive to industrial production use.
[0006] For another example, the Chinese patent application document with publication number CN112547461A discloses a method for coating Teflon on the surface of a mold. Not only does it require corresponding treatment of the mold surface to improve the adhesion of the coating, but it also requires heat treatment of the coating (120-140°C, 60-90 minutes) to improve the strength of the coating. The treatment process is relatively complicated and is not conducive to industrial production and use.
[0007] For example, many Chinese patent application documents with publication numbers such as CN109836939 A, CN108048832 A, CN 115042353A, and CN112547461 A all have the problem of requiring repeated spraying and multiple sintering, and the process is complicated, which is not conducive to industrial production and use.
[0008] Another example is the Chinese patent application document with publication number CN113231598A, which discloses a casting coating and a preparation method thereof. The casting coating includes an independent primer and a surface coating. The raw materials of the primer include, by weight, 100-110 parts of thermal insulation aggregate, 2-20 parts of a first suspending agent, 5-30 parts of a binder, 0.02-0.05 parts of n-butanol, and 200-300 parts of water. The raw materials of the surface coating include, by weight, 100-110 parts of refractory aggregate, 2-30 parts of a second suspending agent, 20-50 parts of aluminum dihydrogen phosphate, 0.02-0.05 parts of n-butanol, and 200-300 parts of water. The method of use is: firstly apply the primer on the surface of the mold to obtain a primer coating, and then apply the surface coating on the surface of the primer coating to form a surface coating; after use, the surface coating can still be intactly attached to the mold plate, and the primer coating is peeled off after the experiment. The casting coating uses two layers of coating, and its operation process is complicated. After the coating is mixed, it needs to be aged for 20 to 26 hours before it can be used. The long time is not conducive to industrial production. Moreover, after use, the bottom coating needs to be peeled off, and the process is very cumbersome.
[0009] In summary, the current traditional mold release coatings have defects such as complicated film-forming process, slow curing speed, high cost, etc. Summary of the invention
[0010] In order to overcome the above problems, the purpose of the present invention is to provide an anti-stick coating for demoulding of refractory prefabricated materials and a preparation method thereof. The anti-stick coating has the characteristics of simple preparation process, simple spraying process, fast curing speed of the anti-stick film, no irritating gas is generated at high temperature, and no anti-stick film remains on the mold after the refractory prefabricated product is demoulded.
[0011] To achieve the above object, the present invention is designed to release a non-stick coating for refractory prefabricated materials, comprising 15 to 50 parts of water glass solution, 3 to 10 parts of refractory aggregate, 3 to 10 parts of hardening accelerator, 0.5 to 1 part of suspending agent, and 10 to 50 parts of water;
[0012] The water glass solution is at least one of liquid sodium water glass, liquid potassium water glass, and liquid potassium sodium water glass;
[0013] The refractory aggregate is corundum or fused magnesia;
[0014] The hardening accelerator is at least one of sodium metaaluminate and calcium aluminate cement;
[0015] The suspending agent is sodium polyacrylate with a relative molecular weight of 1000 to 3000.
[0016] As a preferred embodiment, in the refractory aggregate, the Al2O3 content of corundum is ≥99.0wt%, and the corundum consists of two particle sizes of 0-0.2mm and ≤0.032μm; the MgO content of fused magnesia is ≥97.0wt%, and the fused magnesia consists of two particle sizes of 0-0.2mm and ≤0.032μm.
[0017] As a preferred solution, the weight ratio of the two particle sizes of 0-0.2 mm and ≤0.032 μm in the corundum is 20-30:70-80; the weight ratio of the two particle sizes of 0-0.2 mm and ≤0.032 μm in the fused magnesia is 20-30:70-80.
[0018] As a preferred embodiment, the modulus of the water glass solution is 1.5 to 3.5, and the density is 1.3 to 1.9 g / cm 3 .
[0019] As a preferred solution, the Al2O3 of the calcium aluminate cement is ≥70.0wt%, and the calcium aluminate cement comprises, by weight percentage, 40-70wt% of calcium monoaluminate; less than 25wt% of calcium dialuminate; and less than 3wt% of dodecaluminate heptaaluminate.
[0020] As a preferred embodiment, the hardening accelerator is sodium aluminate and calcium aluminate cement in a weight ratio of 1:1 to 3.
[0021] A method for preparing an anti-sticking coating for demoulding of refractory prefabricated materials comprises the steps of:
[0022] (1) Weighing raw materials: weighing 15-50 parts of water glass solution, 3-10 parts of refractory aggregate, 3-10 parts of hardening accelerator, 0.5-1 part of suspending agent, and 10-50 parts of water by weight;
[0023] (2) Mix water and water glass solution evenly;
[0024] (3) Add refractory aggregate and suspending agent and mix well;
[0025] (4) Add hardening accelerator and mix well.
[0026] The invention discloses an application of an anti-stick coating for demoulding of refractory prefabricated materials. The anti-stick coating for demoulding of refractory prefabricated materials is sprayed or smeared on the inner wall of a refractory prefabricated part mold. After hardening treatment, an anti-stick film with a thickness of 0.2 to 1 mm is formed on the inner wall of the refractory prefabricated part mold. A refractory prefabricated material mixture is injected into the mold. After a curing process, the mold is demoulded. At this time, the anti-stick film has been detached from the inner wall of the mold and adheres to the surface of the product. Then the product enters a drying process. During the drying process, the anti-stick film and the refractory prefabricated material are sintered together.
[0027] The prefabricated material mixture is injected into the mold. The anti-stick coating contains refractory aggregate with a particle size of 0 to 0.2 mm as the anti-stick spray coating skeleton, so that a certain gap is formed between the anti-stick spray coating and the mold. At the same time, a large amount of water is added to the anti-stick spray coating, which will lose water and shrink during the hardening process, which is beneficial to reduce the adhesion between the anti-stick spray coating and the mold and facilitate demoulding. The hardened anti-stick film has high hardness and does not react with the mold. Since the anti-stick coating uses common raw materials for refractory prefabricated materials as the main raw material, it does not produce irritating gases when heated, does not pollute the environment, and is non-toxic and non-corrosive. Its good suspension, dispersibility and easy sintering properties allow the anti-stick coating to sinter with the refractory prefabricated material to form a whole during the drying process of the refractory prefabricated material. Moreover, it is wrapped on the outer surface of the prefabricated material and does not peel or crack at high temperatures, effectively reducing appearance defects such as cavities and bubbles on the surface of the refractory prefabricated material.
[0028] As a preferred solution, when the refractory prefabricated part mold is a small conventional refractory prefabricated part mold, a spraying method is used, and the thickness of the anti-adhesive film is 0.2-0.5 mm. When the refractory prefabricated part mold is large or special-shaped, a smearing method is used, and the thickness of the anti-adhesive film is 0.5-1 mm. The anti-adhesive coating can be hardened at room temperature. According to room temperature changes and production needs, the amount of hardening accelerator added can be adjusted to control the anti-adhesive coating to harden within 1-30 minutes.
[0029] As a preferred solution, the outer surface of the refractory prefabricated material has high flatness after demoulding, with a deviation of less than 0.05 mm.
[0030] The advantages of the present invention are: compared with the traditional ones, the present invention has the following advantages:
[0031] (1) The preparation process of the anti-sticking coating for demoulding of refractory prefabricated materials of the present invention is simple. It only requires a simple mixing of water glass solution, refractory aggregate, hardening accelerator, suspending agent and water. No aging treatment is required, thereby improving the demoulding efficiency of refractory prefabricated materials.
[0032] (2) The spraying process of the anti-sticking coating for demoulding of refractory prefabricated materials of the present invention is simple. It is sufficient to spray or apply an anti-sticking film with a thickness of 0.2 to 1 mm on the inner wall of the mold once, without the need for repeated spraying and application, thereby reducing the thickness of the anti-sticking film and simplifying the spraying process of the anti-sticking coating.
[0033] (3) The anti-sticking coating for demoulding of refractory prefabricated materials of the present invention hardens and forms a film quickly. By adjusting the amount of hardening accelerator added, the coating can be hardened and formed into a film in as fast as 1 minute after spraying or applying. The hardness of the film is high after film formation, and no heat treatment or sintering process is required to improve the strength of the film.
[0034] (4) The anti-sticking film formed after the anti-sticking coating for demoulding of refractory prefabricated materials of the present invention is hardened effectively isolates the mixture from direct contact with the mold during the vibration molding process of the refractory mixture, and effectively solves the problem of refractory prefabricated materials sticking to the mold.
[0035] (5) After the refractory prefabricated material in the mold sprayed with the anti-stick coating for demolding refractory prefabricated materials of the present invention is demolded, the anti-stick coating and the refractory prefabricated material form a whole, completely detach from the inner wall of the mold, do not react with the mold, and do not remain on the mold, thereby reducing the mold cleaning process in the production process and effectively improving production efficiency.
[0036] (6) The anti-sticking coating for demoulding of refractory prefabricated materials of the present invention uses the commonly used raw materials of refractory prefabricated materials as the main raw materials. During the sintering process with the refractory prefabricated materials at a temperature above 300°C, no combustion phenomenon occurs, no irritating gas is generated, safety hazards are avoided, the environment is not polluted, and it is non-toxic and non-corrosive. Its good suspension, dispersibility and easy sintering properties enable the anti-sticking spray coating to be sintered with the refractory prefabricated materials to form a whole during the drying process of the refractory prefabricated materials. It does not peel or crack at high temperatures, and effectively reduces the appearance defects such as cavities and bubbles on the surface of the refractory prefabricated materials.
[0037] (7) The raw materials used in the anti-sticking coating for demoulding of refractory prefabricated materials of the present invention are commonly used raw materials in the production process of refractory materials. The cost is only 1 / 20 of the purchased demoulding agent, which is much lower than the demoulding agent on the market. DETAILED DESCRIPTION
[0038] In order to better understand the present invention, the invention will be described in detail below in conjunction with specific examples.
[0039] The Al2O3 content of the corundum in the following Examples 1 to 5 is ≥ 99.0wt%; the MgO content of the fused magnesia is ≥ 97.0wt%; the Al2O3 of the calcium aluminate cement is ≥ 70.0wt%, and the calcium aluminate cement comprises, by weight percentage, 40 to 70wt% of CA (monocalcium aluminate); CA2 (dialuminate) < 25wt%; C 12 A7 (dodecalcium heptahedralite) < 3 wt%.
[0040] Example 1
[0041] A method for preparing an anti-sticking coating for demoulding of refractory prefabricated materials, comprising the steps of:
[0042] (1) By weight:
[0043] Weigh 15 parts of liquid sodium water glass; modulus is 2.8, density is 1.4g / cm 3 ;
[0044] 10 parts of corundum, of which 2 parts are corundum with a particle size of 0 to 0.2 mm and 8 parts are corundum with a particle size of ≤ 0.032 μm;
[0045] 3 parts sodium aluminate;
[0046] 1 part of sodium polyacrylate with a molecular weight of 1000,
[0047] 10 parts of water, the water is industrial grade circulating water, pH is 7.5;
[0048] (2) mixing water and liquid sodium water glass, and stirring at 2800 r / min for 1 minute to obtain a diluted water glass solution;
[0049] (3) then adding corundum and sodium polyacrylate, stirring at 2800 r / min for 1 minute to obtain a release agent suspension;
[0050] (4) Then, sodium aluminate was added and stirred at 2800 r / min for 1 minute to obtain the desired release agent.
[0051] Example 2
[0052] A method for preparing an anti-sticking coating for demoulding of refractory prefabricated materials, comprising the steps of:
[0053] (1) By weight:
[0054] Weigh 30 parts of liquid potassium water glass, modulus 3.5, density 1.9g / cm 3 ;
[0055] 5 parts of fused magnesia, of which 1 part is fused magnesia with a particle size of 0 to 0.2 mm, and 4 parts are fused magnesia with a particle size of ≤0.032 μm;
[0056] 5 parts of calcium aluminate cement;
[0057] 0.5 parts of sodium polyacrylate with a molecular weight of 2000,
[0058] 20 parts of water, the water is industrial grade circulating water, pH is 8;
[0059] (2) mixing water and liquid potassium water glass, and stirring at 2800 r / min for 2 minutes to obtain a diluted water glass solution;
[0060] (3) then adding fused magnesia and sodium polyacrylate, stirring at 2800 r / min for 2 minutes to obtain a release agent suspension;
[0061] (4) Then add calcium aluminate cement and stir at 2800 r / min for 1 minute to obtain the required release agent.
[0062] Example 3
[0063] A method for preparing an anti-sticking coating for demoulding of refractory prefabricated materials, comprising the steps of:
[0064] (1) By weight:
[0065] Weigh 50 parts of liquid potassium sodium water glass; modulus is 3.0, density is 1.7g / cm 3 ;
[0066] 10 parts of fused magnesia, of which 3 parts are fused magnesia with a particle size of 0 to 0.2 mm and 7 parts are fused magnesia with a particle size of ≤0.032 μm;
[0067] 2.5 parts of sodium aluminate and 7.5 parts of calcium aluminate cement;
[0068] 0.8 parts of sodium polyacrylate with a molecular weight of 3000;
[0069] 50 parts of water, the water is industrial grade circulating water, pH is 7;
[0070] (2) mixing water and liquid potassium sodium water glass, and stirring at 2800 r / min for 2 minutes to obtain a diluted water glass solution;
[0071] (3) then adding fused magnesia and sodium polyacrylate, stirring at 2800 r / min for 2 minutes to obtain a release agent suspension;
[0072] (4) Then, sodium aluminate and calcium aluminate cement were added and stirred at 2800 r / min for 1 minute to obtain the desired release agent.
[0073] Example 4
[0074] A method for preparing an anti-sticking coating for demoulding of refractory prefabricated materials, comprising the steps of:
[0075] (1) By weight:
[0076] Weigh 25 parts of liquid potassium sodium water glass; modulus is 1.5, density is 1.3g / cm 3 ;
[0077] 8 parts of fused magnesia, of which 1.6 parts are fused magnesia with a particle size of 0 to 0.2 mm and 6.4 parts are fused magnesia with a particle size of ≤0.032 μm;
[0078] 4 parts sodium aluminate and 4 parts calcium aluminate cement;
[0079] 1 part of sodium polyacrylate with a molecular weight of 3000;
[0080] 30 parts of water, the water is industrial grade circulating water, pH is 7;
[0081] (2) mixing water and liquid potassium sodium water glass, and stirring at 2800 r / min for 2 minutes to obtain a diluted water glass solution;
[0082] (3) then adding fused magnesia and sodium polyacrylate, stirring at 2800 r / min for 2 minutes to obtain a release agent suspension;
[0083] (4) Then, sodium aluminate and calcium aluminate cement were added and stirred at 2800 r / min for 1 minute to obtain the desired release agent.
[0084] Example 5
[0085] A method for preparing an anti-sticking coating for demoulding of refractory prefabricated materials, comprising the steps of:
[0086] (1) By weight:
[0087] Weigh 40 parts of liquid potassium sodium water glass; modulus is 3.0, density is 1.8g / cm 3 ;
[0088] 3 parts of fused magnesia, of which 0.6 parts are fused magnesia with a particle size of 0 to 0.2 mm and 2.4 parts are fused magnesia with a particle size of ≤0.032 μm;
[0089] 2 parts sodium aluminate and 4 parts calcium aluminate cement;
[0090] 1 part of sodium polyacrylate with a molecular weight of 3000;
[0091] 30 parts of water, the water is industrial grade circulating water, pH is 7;
[0092] (2) mixing water and liquid potassium sodium water glass, and stirring at 2800 r / min for 2 minutes to obtain a diluted water glass solution;
[0093] (3) then adding fused magnesia and sodium polyacrylate, stirring at 2800 r / min for 2 minutes to obtain a release agent suspension;
[0094] (4) Then, sodium aluminate and calcium aluminate cement were added and stirred at 2800 r / min for 1 minute to obtain the desired release agent.
[0095] Test Example 1:
[0096] For small prefabricated materials, the release agent obtained in this embodiment is directly sprayed on the inner wall of the mold, and hardened at room temperature to form a 0.2-0.5 mm anti-sticking film on the inner wall of the mold.
[0097] The anti-stick coating for demoulding of refractory prefabricated materials obtained in Examples 1 to 5 was sprayed on the inner walls of five identical small conventional prefabricated material molds, and the properties of the anti-stick coating were tested as shown in Table 1:
[0098] Table 1
[0099]
[0100] The prefabricated material mixture was injected into five molds sprayed with the anti-sticking coatings of Examples 1 to 5, respectively. The mixture was demoulded after the curing process, and the properties of the refractory prefabricated material and the mold were tested, as shown in Table 2 below:
[0101] Table 2
[0102]
[0103] Test Example 2:
[0104] For large products (unit weight > 100 kg), the release agent obtained in this embodiment can be applied to the inner wall of the mold and allowed to harden at room temperature to form a 0.5-1 mm anti-sticking film on the inner wall of the mold.
[0105] The anti-sticking coating for demoulding of refractory prefabricated materials obtained in Examples 1 to 5 was sprayed on the inner walls of five identical large conventional prefabricated material molds, and the properties of the anti-sticking film were tested as shown in Table 3:
[0106] Table 3
[0107]
[0108] The prefabricated material mixture was injected into five molds sprayed with the anti-sticking coatings of Examples 1 to 5, respectively. The mixture was demoulded after the curing process, and the properties of the refractory prefabricated material and the mold were tested, as shown in Table 4 below:
[0109] Table 4
[0110]
[0111] Test Example 3:
[0112] For special-shaped prefabricated materials, the release agent obtained in this embodiment can be applied to the inner wall of the mold and hardened at room temperature to form a 0.5-1 mm anti-sticking film on the inner wall of the mold.
[0113] The anti-sticking coating for demoulding of refractory prefabricated materials obtained in Examples 1 to 5 was sprayed on the inner walls of five identical special-shaped prefabricated material molds, and the properties of the anti-sticking film were tested as shown in Table 5:
[0114] Table 5
[0115]
[0116] The prefabricated material mixture was injected into five molds sprayed with the anti-sticking coatings of Examples 1 to 5, respectively. The mixture was demoulded after the curing process, and the properties of the refractory prefabricated material and the mold were tested, as shown in Table 6 below:
[0117] Table 6
[0118]
[0119] Based on the above Test Examples 1, 2 and 3, it can be seen that the anti-sticking coating for demoulding the refractory prefabricated materials of Examples 1 to 5 is suitable for various molds. After demoulding, the surface of the refractory prefabricated material is smooth, the porosity of the outer surface is low, and there is no residue on the mold surface.
[0120] The above-mentioned embodiments only express several implementation methods of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the patent of the present invention. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. An application of an anti-sticking coating for demoulding of refractory prefabricated materials, characterized in that: The anti-stick coating for demoulding the refractory prefabricated material is sprayed or applied on the inner wall of the refractory prefabricated part mold. After hardening treatment, an anti-stick film with a thickness of 0.2 to 1 mm is formed on the inner wall of the refractory prefabricated part mold. The refractory prefabricated material mixture is injected into the mold, and the mold is demoulded after the curing process. At this time, the anti-stick film has been separated from the inner wall of the mold and adhered to the surface of the product. Then the product enters the drying process. During the drying process, the anti-stick film and the refractory prefabricated material are sintered together. The anti-sticking coating for demoulding of refractory prefabricated materials comprises, by weight, 15 to 50 parts of water glass solution, 3 to 10 parts of refractory aggregate, 3 to 10 parts of hardening accelerator, 0.5 to 1 part of suspending agent, and 10 to 50 parts of water; The water glass solution is at least one of liquid sodium water glass, liquid potassium water glass, and liquid potassium sodium water glass; The refractory aggregate is corundum or fused magnesia; The hardening accelerator is at least one of sodium metaaluminate and calcium aluminate cement; The suspending agent is sodium polyacrylate with a relative molecular weight of 1000 to 3000.
2. The use of the anti-sticking coating for demoulding of refractory prefabricated materials according to claim 1, characterized in that: When the refractory prefabricated part mold is a small conventional refractory prefabricated part mold, a spraying method is adopted, the thickness of the anti-sticking film is 0.2-0.5mm, the hardening treatment time is 1-20 minutes, the hardness of the anti-sticking film is 6H, the thickness uniformity of the anti-sticking film after hardening is within 20um, and the strength of the anti-sticking film is 1.2-2.4MPa; when the refractory prefabricated part mold is a large or special-shaped refractory prefabricated part mold, a smearing method is adopted, the thickness of the anti-sticking film is 0.5-1mm, the hardening treatment is placed at room temperature for 19-30 minutes, the hardness of the anti-sticking film is 6H, the thickness uniformity of the anti-sticking film after hardening is within 40um, and the strength of the anti-sticking film is 1.3-2.6MPa.
3. The use of the anti-sticking coating for demoulding of refractory prefabricated materials according to claim 1, characterized in that: After the refractory prefabricated material is dried, the surface porosity is 4.0-7.9% and the flatness is less than 0.05 mm.