A method for improving blast furnace charging efficiency

The multi-ring matrix charging method optimizes blast furnace gas flow distribution by distributing coke and ore in specific zones, addressing gas utilization and fuel consumption issues, and ensuring stable furnace operation with inferior raw materials.

CN116179772BActive Publication Date: 2024-12-03ANGANG STEEL CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310167182.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-27
Publication Date
2024-12-03
Estimated Expiration
2043-02-27

AI Technical Summary

Technical Problem

Existing blast furnace charging methods face challenges in achieving high gas utilization rates and reducing fuel consumption while maintaining stable operation, particularly when using inferior raw materials, due to issues with gas flow distribution and coke accumulation in the furnace center.

Method used

A multi-ring matrix charging method is employed, distributing 20-30% of coke in the secondary edge area and ore evenly in the edge, middle, and secondary center belts of the furnace throat, with specific gear settings and laser scanning to optimize material flow angles and widths, ensuring a stable gas passage and even gas distribution.

Benefits of technology

This method enhances gas permeability, improves adaptability to inferior raw materials, prevents coke accumulation, and reduces fuel consumption by ensuring even gas flow and stable furnace operation, thereby increasing gas utilization and production capacity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004096273900000061
    Figure BDA0004096273900000061
  • Figure BDA0004096273900000071
    Figure BDA0004096273900000071
Patent Text Reader

Abstract

The present invention relates to a blast furnace charging method for improving gas utilization. The method adopts a multi-ring matrix charging method, and 20% to 30% of coke is charged in the secondary edge area of ​​the furnace throat. At the same time, the ore is evenly distributed in the edge, middle annular belt and secondary center belt of the furnace throat, so that the charging amount of coke and ore in the secondary edge area is greater than that in other areas, forming a gas flow distribution with the secondary edge area of ​​the furnace throat as the main part and the center of the furnace throat as the auxiliary part. A stable gas passage is formed in the secondary edge annular belt of the blast furnace, which ensures the gas permeability of the blast furnace; at the same time, the accumulation phenomenon in the center of the furnace cylinder is avoided, so as to ensure the stable and smooth operation of the blast furnace and improve the production capacity; the large angle difference charging method is adopted to evenly distribute the gas flow inside the blast furnace, thereby improving the gas utilization rate and reducing the fuel consumption of the blast furnace.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of blast furnace smelting, and in particular to a blast furnace charging method for improving gas utilization. Background Art

[0002] At present, there are two main ways of charging for large and medium-sized blast furnaces that use bellless top equipment and multi-ring charging systems: one is with center coking and the other is without center coking. The purpose of center coking is to increase the proportion of coke in the center of the blast furnace, reduce the resistance of the charge in the center to the blast furnace gas, and thus reduce the slow descent speed and stagnation of the charge caused by the high resistance of the charge to the blast furnace gas, which is not conducive to the smooth operation of the blast furnace, so as to achieve blast furnace stability and high production. However, after the center coke is added to the charge, the resistance of the charge in the center to the gas in the furnace is reduced, which will lead to an increase in the gas flow rate in the center of the furnace, shortening the contact time between the gas and the charge, thereby reducing the amount of iron oxides in the charge reduced by the gas. Therefore, blast furnaces with center coke addition generally have lower gas utilization and higher fuel consumption. In addition, when the center coke addition ratio of the blast furnace is too high, a large proportion of the center coke will fall into the furnace, and the deterioration of the coke will cause the particle size of the coke in the center of the furnace to drop sharply, thereby reducing the air and liquid permeability of the coke in the core of the furnace, which can easily cause accumulation in the blast furnace and cause periodic deterioration of the technical and economic indicators of the blast furnace.

[0003] The blast furnace without central coking has high gas utilization rate and low fuel ratio, but because it cannot form a gas channel without mining area in the center of the blast furnace like the central coking distribution method, the blast furnace pressure difference is often very high; this distribution method is only suitable for blast furnaces with high-quality raw and fuel conditions.

[0004] Therefore, it is urgent to invent a new charging method which has the advantages of good air permeability and strong adaptability to raw materials and fuels of the charging method with center-coking, and the advantage of low fuel consumption of the charging method without center-coking.

[0005] In recent years, as steel companies pay more and more attention to increasing the production and reducing the consumption of blast furnaces, several bell-less furnace top multi-ring matrix distribution methods have emerged, such as:

[0006] The Chinese patent application with application number 201010197018.7 discloses a "multi-ring matrix distribution center coke adding method for blast furnace bellless top". Based on the multi-ring matrix distribution method, more than 50% of the coke is first distributed in the center area of ​​the furnace throat, so that the thickness of the central coke is greater than the thickness of the edge coke, so that the throat material surface is in the shape of a steamed bun; because the center of the material surface is high and the edge is low, the mixed material layer in the center of the furnace throat is eliminated, thereby achieving precise control of the radial ore-coke ratio. The advantage is that it can adapt to the fluctuation of coke quality and is conducive to the use of small-size ore, keeping the furnace condition stable and smooth, achieving the purpose of stabilizing the edge and opening the center, thereby reducing production costs. The edge temperature of the furnace top thermal imaging is 120±50℃, and the center temperature is 450±150℃.

[0007] The Chinese patent application with application number 201611172876.X discloses a "blast furnace charging method that adapts to different furnace conditions and achieves efficient smelting", which includes the following steps: 1) Divide the equal area of ​​the material surface into several equal parts, and measure the actual corresponding charging angle and material flow angle of each equal part; 2) Charging the charging at the center, and the amount of charging at the center is 20-25% of the total coke amount; 3) Coke, large sintered ore and small sintered ore are distributed in two or more ways, including the same angle distribution, staggered angle distribution and the same angle staggered angle distribution, and the distribution width is 1-5 angles. The blast furnace charging method implements graded feeding according to the sintered ore to change the charging method and the amount of coke added at the center of coke, large sintered ore and small sintered ore, and control the gas flow distribution. It can be applied to the situation where the raw material and fuel conditions change greatly and the furnace conditions often fluctuate, and ensure the smooth implementation of the blast furnace.

[0008] The Chinese patent application with application number 201710492105.7 discloses a method for radial coke load distribution in the throat of a blast furnace. The method controls the coke load distribution of the radial segment of the throat as follows: the coke load distribution corresponding to the 0.8-1.0m ring belt portion at the edge of the throat of the furnace is controlled to be 0.90 to 1.05 times the coke load entering the furnace, the coke load distribution corresponding to the 1.0 to 2.0m width portion of the middle ring belt is 1.30 to 1.50 times the coke load entering the furnace, and the coke load distribution corresponding to the 2.5 to 3.0m width portion of the central funnel ring belt is 0.60 to 0.80 times the coke load entering the furnace. When the blast furnace is performing central coking production, the central coking angle is generally controlled at 8° to 15°, and the central coking amount is preferably controlled at 15% to 25% of the coke batch. The method is used for blast furnace production operation, the blast furnace operation cost is low, the blast furnace production is stable, and the coke ratio can be reduced by 10 to 15 kg / t.

[0009] The Chinese patent application with application number 202010072322.2 discloses a "Method for compensating coke addition in the center of a bellless distribution system", which includes the following steps: 1) Calculate the total number of coke distribution cycles, total time, and coke distribution weight speed per second for each coke distribution system; 2) Calculate the amount of coke added in the center; 3) Determine the inclination angle of the innermost ring chute of the coke in the specific distribution system; 4) Calculate the amount of coke added in the center. Its advantages are: the size of the coke pile in the center area of ​​the furnace top is fixed, the center gas flow is stabilized, and the blast furnace condition is maintained stable and smooth; the radial O / C distribution reaches the design target, the material surface shape is stable, and there is no ore rolling into the center.

[0010] Although the above-mentioned center coking and charging method can be applied to blast furnaces with poor raw material conditions, so that the blast furnace can ensure stable and smooth operation while using low-cost and inferior raw materials, the center coking and charging method will cause the gas flow rate in the center of the furnace to increase, shorten the contact time between the gas and the charge, and increase the fuel consumption of the blast furnace.

[0011] The article "The Practice of Canceling Center Coking in Ma Steel's No. 4 Blast Furnace" (Ironmaking, Issue 2, 2019) proposes a method of distributing materials without center coking. Although this method can effectively reduce fuel consumption, the blast furnace using this method must be matched with high-quality raw materials, and the corresponding raw material costs are also relatively high. Summary of the invention

[0012] The present invention provides a blast furnace charging method for improving gas utilization, forming a stable gas passage in an annular belt at the secondary edge of the blast furnace, thereby ensuring the air permeability of the blast furnace; at the same time, avoiding the accumulation phenomenon in the center of the furnace, ensuring the stable and smooth operation of the blast furnace and improving the production capacity; adopting large-angle differential charging to make the gas flow evenly distributed inside the blast furnace, thereby improving the gas utilization rate and reducing the fuel consumption of the blast furnace.

[0013] In order to achieve the above object, the present invention adopts the following technical solutions:

[0014] A blast furnace charging method for improving gas utilization rate adopts a multi-ring matrix charging method, 20% to 30% of coke is distributed in the secondary edge area of ​​the furnace throat, and ore is evenly distributed in the edge, middle ring belt and secondary center belt of the furnace throat, so that the charging amount of coke and ore in the secondary edge area is greater than that in other areas, forming a gas flow distribution with the secondary edge area of ​​the furnace throat as the main area and the center of the furnace throat as the auxiliary area.

[0015] Furthermore, when setting the fabric matrix, 7 gears are set; among them, gear 7# corresponds to the edge ring belt, gear 6# corresponds to the secondary edge ring belt, gears 4# to 5# correspond to the middle ring belt, gears 2# to 3# correspond to the secondary center belt, and gear 1# corresponds to the center area.

[0016] Furthermore, the manhole of the blast furnace is opened when the furnace is opened for charging, and the material flow width d, material flow trajectory and material distribution angle ɑ at different gears are determined by laser scanning according to the principle that the material flows at each gear do not interfere with each other; the details are as follows:

[0017] ① According to the principle that the outer trajectory of the 7# gear flow is tangent to the throat steel brick, determine the distribution angle ɑ7 and the corresponding material flow width d7 of the 7# gear;

[0018] ② According to the principle that the distance between the outer charge landing point of the 6# gear flow and the inner charge landing point of the 7# gear flow is 0.1-0.2m, determine the distribution angle ɑ6 of the 6# gear and the corresponding material flow width d6;

[0019] ③ According to the principle that the distance between the outer charge point of the 5# gear flow and the inner charge point of the 6# gear flow is 0.1-0.2m, determine the distribution angle ɑ5 of the 5# gear and the corresponding material flow width d5;

[0020] ④ According to the principle that the radius of the charge point on the outside of the 4# gear flow is the same as the radius of the charge point on the inside of the 5# gear flow, determine the distribution angle ɑ4 of the 4# gear and the corresponding flow width d4;

[0021] ⑤ According to the principle that the radius of the charge point on the outside of the 3# gear flow is the same as the radius of the charge point on the inside of the 4# gear flow, determine the distribution angle ɑ3 of the 3# gear and the corresponding flow width d3;

[0022] ⑥ According to the principle that the radius of the charge point on the outside of the 2# gear flow is the same as the radius of the charge point on the inside of the 3# gear flow, determine the distribution angle ɑ2 of the 2# gear and the corresponding flow width d2;

[0023] ⑦The fabric angle ɑ1 of gear position 1# is 0°.

[0024] Furthermore, when the distribution matrix is ​​used for distribution, coke is distributed in all 7 gears, and ore is distributed in 5 gears, namely, gears 2# to 5# and gear 7#, that is, ore is not distributed in the secondary edge area and the center area of ​​the furnace throat.

[0025] Furthermore, the coke distribution process is as follows: 20% to 30% of the coke in the trough is distributed at the 6# gear, i.e., the secondary edge area of ​​the furnace throat; 5% to 10% of the coke in the trough is distributed at the 1# gear, i.e., the center of the furnace throat; and the remaining coke in the trough is evenly distributed at the 7# gear, 5# gear, 4# gear, 3# gear and 2# gear.

[0026] Furthermore, the ore feeding process is as follows: starting from the 7# gear, after the 7# gear is fed, the discharge gate is closed and no more ore is fed into the blast furnace, the trough is tilted to the 5# gear, and then the discharge gate is reopened to feed the ore into the blast furnace; the ore is evenly distributed at the 7# gear, 5# gear, 4# gear, 3# gear and 2# gear.

[0027] Further, the batch weight W of the coke 焦 for:

[0028] Furthermore, the ore and coke are distributed at the same angle, wherein the total angle difference of the ore is 18° to 25°, and the total angle difference of the coke is 35° to 45°.

[0029] Furthermore, the blast furnace blast kinetic energy is controlled at 85-100 kJ / s, and the actual blast furnace wind speed is controlled at 210-230 m / s.

[0030] Compared with the prior art, the present invention has the following beneficial effects:

[0031] (1) A stable gas passage can be formed in the annular zone at the secondary edge of the blast furnace, thereby ensuring the gas permeability of the blast furnace and further improving the blast furnace's adaptability to inferior raw materials and fuels;

[0032] (2) Compared with blast furnaces using traditional charging methods, this method can avoid the accumulation of coke in the center of the furnace caused by the rapid decrease in the particle size of coke in the center of the furnace due to the deterioration of coke after entering the furnace, thereby ensuring the stable and smooth operation of the blast furnace and improving production capacity;

[0033] (3) The use of large angle difference distribution can make the gas flow evenly distributed inside the blast furnace, thereby improving the gas utilization rate and reducing the blast furnace fuel consumption. DETAILED DESCRIPTION

[0034] A blast furnace charging method for improving gas utilization rate disclosed in the present invention adopts a multi-ring matrix charging method to charge 20% to 30% of coke in the secondary edge area of ​​the furnace throat, and at the same time evenly distributes ore in the edge, middle annular belt and secondary center belt of the furnace throat, so that the charging amount of coke and ore in the secondary edge area is greater than that in other areas, forming a gas flow distribution with the secondary edge area of ​​the furnace throat as the main part and the center of the furnace throat as the auxiliary part.

[0035] Furthermore, when setting the fabric matrix, 7 gears are set; among them, gear 7# corresponds to the edge ring belt, gear 6# corresponds to the secondary edge ring belt, gears 4# to 5# correspond to the middle ring belt, gears 2# to 3# correspond to the secondary center belt, and gear 1# corresponds to the center area.

[0036] Furthermore, the manhole of the blast furnace is opened when the furnace is opened for charging, and the material flow width d, material flow trajectory and material distribution angle ɑ at different gears are determined by laser scanning according to the principle that the material flows at each gear do not interfere with each other; the details are as follows:

[0037] ① According to the principle that the outer trajectory of the 7# gear flow is tangent to the throat steel brick, determine the distribution angle ɑ7 and the corresponding material flow width d7 of the 7# gear;

[0038] ② According to the principle that the distance between the outer charge landing point of the 6# gear flow and the inner charge landing point of the 7# gear flow is 0.1-0.2m, determine the distribution angle ɑ6 of the 6# gear and the corresponding material flow width d6;

[0039] ③ According to the principle that the distance between the outer charge point of the 5# gear flow and the inner charge point of the 6# gear flow is 0.1-0.2m, determine the distribution angle ɑ5 of the 5# gear and the corresponding material flow width d5;

[0040] ④ According to the principle that the radius of the charge point on the outside of the 4# gear flow is the same as the radius of the charge point on the inside of the 5# gear flow, determine the distribution angle ɑ4 of the 4# gear and the corresponding flow width d4;

[0041] ⑤ According to the principle that the radius of the charge point on the outside of the 3# gear flow is the same as the radius of the charge point on the inside of the 4# gear flow, determine the distribution angle ɑ3 of the 3# gear and the corresponding flow width d3;

[0042] ⑥ According to the principle that the radius of the charge point on the outside of the 2# gear flow is the same as the radius of the charge point on the inside of the 3# gear flow, determine the distribution angle ɑ2 of the 2# gear and the corresponding flow width d2;

[0043] ⑦The fabric angle ɑ1 of gear position 1# is 0°.

[0044] Furthermore, when the distribution matrix is ​​used for distribution, coke is distributed in all 7 gears, and ore is distributed in 5 gears, namely, gears 2# to 5# and gear 7#, that is, ore is not distributed in the secondary edge area and the center area of ​​the furnace throat.

[0045] Furthermore, the coke distribution process is as follows: 20% to 30% of the coke in the trough is distributed at the 6# gear, i.e., the secondary edge area of ​​the furnace throat; 5% to 10% of the coke in the trough is distributed at the 1# gear, i.e., the center of the furnace throat; and the remaining coke in the trough is evenly distributed at the 7# gear, 5# gear, 4# gear, 3# gear and 2# gear.

[0046] Furthermore, the ore feeding process is as follows: starting from the 7# gear, after the 7# gear is fed, the discharge gate is closed and no more ore is fed into the blast furnace, the trough is tilted to the 5# gear, and then the discharge gate is reopened to feed the ore into the blast furnace; the ore is evenly distributed at the 7# gear, 5# gear, 4# gear, 3# gear and 2# gear.

[0047] Further, the batch weight W of the coke 焦 for:

[0048] Furthermore, the ore and coke are distributed at the same angle, wherein the total angle difference of the ore is 18° to 25°, and the total angle difference of the coke is 35° to 45°.

[0049] Furthermore, the blast furnace blast kinetic energy is controlled at 85-100 kJ / s, and the actual blast furnace wind speed is controlled at 210-230 m / s.

[0050] The following embodiments are implemented on the premise of the technical solution of the present invention, and detailed implementation methods and specific operation processes are given, but the protection scope of the present invention is not limited to the following embodiments. It should also be noted that the technical features or combinations of technical features described in the following embodiments should not be considered isolated, and they must be combined with each other to achieve better technical effects.

[0051] [Example 1]

[0052] In this embodiment, the volume is 3200m 3 Taking the blast furnace of as an example, its throat diameter is 4.5m, the waist diameter is 13.7m, and the batch weight of coke is 27.1t.

[0053] 1. Setting of the material distribution matrix: According to the 7-gear setting, the blast furnace manhole is opened when the furnace is opened for charging. The material flow width d, material flow trajectory and material distribution angle ɑ (see Table 1 for details) are determined at different ring positions by laser scanning according to the principle that the material flows at each gear do not interfere with each other. The details are as follows:

[0054] ① According to the principle that the outer trajectory of the material flow at the outermost ring 7# gear is tangent to the throat steel brick, the material distribution angle ɑ7 of the outermost ring 7# gear is determined to be 43°, and the corresponding material flow width d7 is 0.75m;

[0055] ② Determine the material distribution angle ɑ6 of the 6# gear as 39.1°, and the corresponding material flow width d6 is 0.69m;

[0056] ③ Determine the material distribution angle ɑ5 of the 5# gear as 34.4°, and the corresponding material flow width d5 ​​is 0.65m;

[0057] ④ Determine the material distribution angle ɑ4 of the 4# gear to be 31.1°, and the corresponding material flow width d4 to be 0.6m;

[0058] ⑤ Determine the material distribution angle ɑ3 of the 3# gear as 27.1°, and the corresponding material flow width d3 is 0.55m;

[0059] ⑥ Determine that the material distribution angle ɑ2 of the 2# gear is 22.8°, and the corresponding material flow width d2 is 0.53m;

[0060] ⑦ The fabric angle ɑ1 of the center focus 1# position is 0°

[0061] Table 1 Blast furnace burden distribution position, material flow width and angle

[0062]

[0063] 2. The blast furnace adopts the following charging system:

[0064] When distributing coke, the total number of coke distribution circles is 2+3+2+2+2+2+1=14 circles. 21.4% of the total amount of coke in the trough is evenly distributed on the secondary edge zone (i.e., the 6# gear), 7.14% of the total amount of coke in the trough is distributed in the center of the blast furnace (i.e., the 1# gear), and the remaining coke is evenly distributed on 5 gears, namely, 7#, 5#, 4#, 3# and 2# (see Table 2).

[0065] Table 2 Coke distribution matrix

[0066] Fabric gear 7# 6# 5# 4# 3# 2# 1# Number of coke distribution circles (circles) 2 3 2 2 2 2 1

[0067] When the ore is distributed, the total number of ore distribution circles is 2+0+2+2+2+2+0=10 circles, and the ore in the trough is evenly distributed on the 5 gears of 7#, 5#, 4#, 3# and 2#. The specific operation method is: start distributing from the 7# gear at the edge, close the discharge gate after the distribution of the 7# gear is completed, keep the ore weight in the weighing tank unchanged, and stop distributing to the blast furnace. When the trough tilts to the 5# gear, reopen the discharge gate to distribute the ore inside the blast furnace (see Table 3).

[0068] Table 3 Ore distribution matrix

[0069] Fabric gear 7# 6# 5# 4# 3# 2# 1# ore 2 0 2 2 2 2 0

[0070] 3. The kinetic energy of blast furnace air is controlled at 90kJ / s and the wind speed is 218m / s.

[0071] In this embodiment, the gas utilization rate of the blast furnace is increased by 2.3% compared with that before implementation. The comparison of various indicators of the blast furnace before and after implementation is as follows (see Table 4).

[0072] Table 4 Comparison of blast furnace indicators

[0073] time Gas utilization rate, % Fuel ratio, kg / t Average daily output, t / d Wind pressure, kPa Top pressure, kPa Pressure difference, kPa Before implementation 46 570 7000 386 213 173 After implementation 48.3 543 7800 396 221 175

[0074] [Example 2]

[0075] The present invention has a volume of 2580m 3 Taking the blast furnace of as an example, its throat diameter is 4.2m, the waist diameter is 13m, and the coke batch weight is 22t.

[0076] 1. Setting of the material distribution matrix: According to the 7-gear setting, the blast furnace manhole is opened when the furnace is opened for charging. The laser scanning method is used to determine the material flow width d, material flow trajectory and material distribution angle ɑ (see Table 5) when distributing materials at different ring positions according to the principle that the material flows at each gear do not interfere with each other. The details are as follows:

[0077] ① According to the principle that the outer trajectory of the material flow at the outermost ring 7# gear is tangent to the throat steel brick, the material distribution angle ɑ7 of the outermost ring 7# gear is determined to be 40°, and the corresponding material flow width d7 is 0.67m;

[0078] ② Determine the material distribution angle ɑ6 of the 6# gear to be 36°, and the corresponding material flow width d6 to be 0.59m;

[0079] ③ Determine the material distribution angle ɑ5 of the 5# gear as 31.3°, and the corresponding material flow width d5 ​​is 0.52m;

[0080] ④ Determine the material distribution angle ɑ4 of the 4# gear to be 28°, and the corresponding material flow width d4 to be 0.49m;

[0081] ⑤ Determine the material distribution angle ɑ3 of the 3# gear as 24°, and the corresponding material flow width d3 is 0.45m;

[0082] ⑥ Determine the material distribution angle ɑ2 of the 2# gear as 19.6°, and the corresponding material flow width d2 is 0.39m;

[0083] ⑦ The fabric angle ɑ1 of the center focus 1# position is 0°

[0084] Table 5 Blast furnace distribution gear, material flow width and angle

[0085]

[0086] 2. The blast furnace adopts the following charging system:

[0087] When distributing coke, the total number of coke distribution circles is 3+4+3+3+3+3+1=20 circles. 20% of the total coke in the trough is evenly distributed on the secondary edge zone (i.e. 6# gear), 5% of the total coke in the trough is distributed in the center of the blast furnace (i.e. 1# gear), and the remaining coke is evenly distributed on 5 gears, namely 7#, 5#, 4#, 3# and 2# (see Table 6).

[0088] Table 6 Coke distribution matrix

[0089] Fabric gear 7# 6# 5# 4# 3# 2# 1# Number of coke distribution circles (circles) 3 4 3 3 3 3 1

[0090] When ore is distributed, the total number of ore distribution circles is 3+0+3+3+3+3+0=15 circles, and the ore in the trough is evenly distributed on 5 gears, namely 7#, 5#, 4#, 3# and 2#. The specific operation method is: start distributing from the 7# gear at the edge, close the discharge gate after distributing the 7# gear, keep the ore weight in the weighing tank unchanged, and stop distributing to the blast furnace. When the trough tilts to the 5# gear, reopen the discharge gate to distribute the ore inside the blast furnace (see Table 7);

[0091] Table 7 Ore distribution matrix

[0092] Fabric gear 7# 6# 5# 4# 3# 2# 1# ore 3 0 3 3 3 3 0

[0093] 3. The blast furnace blast energy is controlled at 96kJ / s and the wind speed is 222m / s;

[0094] In this embodiment, the coke in the blast furnace is reduced by 2.3% compared with that before implementation. The comparison of various indicators of the blast furnace before and after implementation is as follows (see Table 8).

[0095] Table 8 Blast furnace index comparison

[0096] time Gas utilization rate, % Fuel ratio, kg / t Average daily output, t / d Wind pressure, kPa Top pressure, kPa Pressure difference, kPa Before implementation 47 550 5600 397 172 225 After implementation 50.3 503 6300 403 179 224

[0097] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A blast furnace charging method for improving gas utilization, characterized in that: A multi-ring matrix distribution method is adopted to distribute 20% to 30% of coke in the secondary edge area of ​​the furnace throat, and at the same time, the ore is evenly distributed in the edge, middle ring belt and secondary center belt of the furnace throat, so that the distribution amount of coke and ore in the secondary edge area is greater than that in other areas, forming a gas flow distribution with the secondary edge area of ​​the furnace throat as the main area and the center of the furnace throat as the auxiliary area. When setting the distribution matrix, it is set according to 7 gears; among them, the 7# gear corresponds to the edge ring belt, the 6# gear corresponds to the secondary edge ring belt, the 4#~5# gears correspond to the middle ring belt, the 2#~3# gears correspond to the secondary center belt, and the 1# gear corresponds to the center area; when the distribution matrix is ​​applied, coke is distributed in all 7 gears, and the ore is distributed in 5 gears including the 2#~5# gear and the 7# gear, that is, the ore is not distributed in the secondary edge area and the center area of ​​the furnace throat; The coke distribution process is as follows: 20% to 30% of the coke in the trough is distributed in the 6# gear, i.e., the secondary edge area of ​​the furnace throat; 5% to 10% of the coke in the trough is distributed in the 1# gear, i.e., the center of the furnace throat; the remaining coke in the trough is evenly distributed in the 7# gear, 5# gear, 4# gear, 3# gear, and 2# gear; The ore distribution process is as follows: starting from the 7# gear, after the 7# gear is distributed, the discharge gate is closed and no more ore is distributed into the blast furnace, the trough is tilted to the 5# gear, and then the discharge gate is reopened to distribute ore into the blast furnace; the ore is distributed evenly in the 7# gear, 5# gear, 4# gear, 3# gear and 2# gear; The blast furnace blast kinetic energy is controlled at 85-100 kJ / s, and the actual blast furnace wind speed is controlled at 210-230 m / s.

2. A blast furnace charge distribution method for improving gas utilization efficiency according to claim 1, characterized in that: The manhole of the blast furnace is opened when the furnace is opened for charging. The material flow width d, material flow trajectory and material distribution angle ɑ at different gears are determined by laser scanning according to the principle that the material flows at each gear do not interfere with each other. The details are as follows: ① According to the principle that the outer trajectory of the 7# gear flow is tangent to the throat steel brick, determine the distribution angle ɑ7 and the corresponding material flow width d7 of the 7# gear; ② According to the principle that the distance between the outer charge point of the 6# gear flow and the inner charge point of the 7# gear flow is 0.1-0.2m, determine the distribution angle ɑ6 of the 6# gear and the corresponding material flow width d6; ③ According to the principle that the distance between the outer charge point of the 5# gear flow and the inner charge point of the 6# gear flow is 0.1-0.2m, determine the distribution angle ɑ5 of the 5# gear and the corresponding material flow width d5; ④ According to the principle that the radius of the charge point on the outside of the 4# gear flow is the same as the radius of the charge point on the inside of the 5# gear flow, determine the distribution angle ɑ4 of the 4# gear and the corresponding flow width d4; ⑤ According to the principle that the radius of the charge point on the outside of the 3# gear flow is the same as the radius of the charge point on the inside of the 4# gear flow, determine the distribution angle ɑ3 of the 3# gear and the corresponding flow width d3; ⑥ According to the principle that the radius of the charge point on the outside of the 2# gear flow is the same as the radius of the charge point on the inside of the 3# gear flow, determine the distribution angle ɑ2 of the 2# gear and the corresponding flow width d2; ⑦ The fabric angle ɑ1 of 1# gear is 0°.

3. A blast furnace charge distribution method for improving gas utilization efficiency according to claim 1, characterized in that: The batch weight of the coke is W 焦 for: .

4. A blast furnace charging method for improving gas utilization efficiency according to claim 1, characterized in that: The ore and coke are distributed at the same angle, wherein the total angle difference of the ore is 18° to 25°, and the total angle difference of the coke is 35° to 45°.