A high-efficiency soft-touch wet friction fastness enhancer and preparation method thereof
The wet rubbing fastness improving agent prepared through specific combinations and reaction steps solves the problems of hardening and stability of the hand feel in the existing technology, improves the wet rubbing fastness and hand feel of the fabric, and reduces the harm to the human body.
Patent Information
- Application Number
- CN202211628574.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-17
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2042-12-17
AI Technical Summary
Existing wet rubbing fastness improving agents have problems such as hardening of the hand, stability problems and great harm to the human body during use, and the wet rubbing fastness improving effect is not obvious.
Use 40-100 parts of polyether, 10-30 parts of tristyrylphenol polyoxyethylene ether, 40-100 parts of solvent, 60-120 parts of isocyanate, 0.5-4 parts of active hydrogenated compound containing tertiary amino groups, 40- A combination of 80 parts of hydroxyl silicone oil, 600-800 parts of deionized water, 0.5-3 parts of diamine chain extender, and 0.5-5 parts of acid is used to prepare a high-efficiency, soft-feel wet rubbing fastness enhancer through specific reaction steps.
It achieves a significant improvement in the wet rubbing fastness of the fabric and a softer feel, while improving the stability of the product and reducing the harm to the human body.
Abstract
Description
Technical Field
[0001] The invention relates to a high-energy-efficiency soft-hand wet friction fastness enhancer and a preparation method thereof, belonging to the technical field of textile printing and dyeing auxiliaries. Background Art
[0002] Reactive dyes have a complete color spectrum, good dyeing permeability, low dyeing cost, short dyeing time, easy use, and bright color. They are the preferred dyes for dyeing cellulose fabrics. Although reactive dyes can form covalent bonds with fibers, the color fastness of cotton and its blended fabrics dyed with them is not satisfactory, especially the washing fastness and wet rubbing fastness. It is often necessary to add wet rubbing fastness improvers to fix the dyed fabrics. In recent years, water-based polyurethane has been used more and more widely in the textile industry, and its proportion has increased. Water-based polyurethane can be used as waterproofing agent, wool shrink-proof finishing agent, fabric non-ironing finishing agent, synthetic fiber hydrophilic and antistatic agent, anti-pilling agent and wet rubbing fastness improver.
[0003] At present, the research on wet friction fastness enhancers for reactive dye-dyed cotton fabrics is mainly based on water-based polyurethanes, such as a patent for a long-lasting wet friction fastness enhancer and its preparation method (application number CN201110272757.2), which includes polyisocyanate compounds, polyether polyol compounds, small molecule chain extenders, blocking agents and neutralizing acids, and the contents of each component are calculated by mass: 10-40 parts of polyisocyanate compounds; 50-90 parts of polyether polyol compounds; 0.5-10 parts of small molecule chain extenders; 0.5-10 parts of blocking agents; 0.5-5 parts of neutralizing acids. The invention actually produces cationic reactive water-based polyurethane, but the product synthesized in the patent has limited improvement in wet friction fastness during use, and the fabric feels hard after treatment, which has a great impact on the feel, and needs to be supplemented with additional softeners.
[0004] Therefore, wet friction fastness enhancers of silicone-modified polyurethanes have emerged in the market. For example, the patent of an environmentally friendly polyether silicone-modified polyurethane and its preparation method (application number CN201710181730.X) discloses 5 to 10 parts of polyether silicone, 10 to 50 parts of chain extenders, 10 to 50 parts of polyols, 20 to 60 parts of isocyanate compounds, 10 to 20 parts of diacryl acetal pentaerythritol, 5 to 15 parts of 4-allyl-1,2-dimethoxybenzene, and 2 to 10 parts of 1-allyl-3-methoxy-4-hydroxybenzene; wherein the chain extender is 1,4-butanediol and a chain extender containing quaternary ammonium salt; the chain extender containing quaternary ammonium salt is obtained by copolymerization of pentaerythritol and quaternary ammonium salt monomers, and the quaternary ammonium salt monomers include one or more of acryloyloxyethyl alkyl quaternary ammonium salt and allyl alkyl quaternary ammonium salt.
[0005] Although the introduction of silicone into polyurethane can give the fabric a good soft feel, it is prone to stability problems such as sticking to the roller, demulsification, and silicon spots on the fabric during the processing process, and the effect of improving wet friction fastness is not obvious; moreover, most of the current wet friction fastness improvers use TDI as a synthetic raw material, TDI is highly toxic, and the residual TDI is very harmful to the human body. Summary of the invention
[0006] In view of the problems existing in the above-mentioned prior art, the present invention provides a high-efficiency soft-hand wet friction fastness improving agent and a preparation method thereof, which has a soft hand feel, obvious wet friction fastness improving effect, good stability and little harm to the human body.
[0007] In order to achieve the above-mentioned purpose, the invention adopts a high-efficiency soft-hand wet friction fastness enhancer, which comprises the following raw materials, by weight: 40-100 parts of polyether, 10-30 parts of tristyrylphenol polyoxyethylene ether 16EO, 40-100 parts of solvent, 60-120 parts of isocyanate, 0.5-4 parts of active hydride containing tertiary amino group, 40-80 parts of hydroxy silicone oil, 600-800 parts of deionized water, 0.5-3 parts of diamine chain extender, and 0.5-5 parts of acid.
[0008] As an improvement, the polyether is at least one of PEG1000, PEG2000, and PTMEG2000.
[0009] As an improvement, one of the polyethers is tristyrylphenol polyoxyethylene ether 16EO.
[0010] As an improvement, the solvent is at least one of dimethylformamide, tetrahydrofuran, N-methyl-2-pyrrolidone, toluene, propylene glycol monomethyl ether acetate, butanone, and acetone.
[0011] As an improvement, the isocyanate polymer is at least one of TDI polymer DESMODUR L75, HDI polymer DESMODURN100 and HDI polymer DESMODURN3300.
[0012] As an improvement, the active hydrogenated compound containing tertiary amino groups is at least one of N,N-dimethylethanolamine, N-methyldiethanolamine, N,N-dimethylethylenediamine and triethanolamine.
[0013] As an improvement, the hydroxy silicone oil adopts at least one of the double-terminal hydroxy silicone oils with a molecular weight of 1000-10000.
[0014] As an improvement, the diamine type chain extender is at least one of ethylenediamine, o-phenylenediamine, hydrazine hydrate and isophoronediamine.
[0015] As an improvement, the acid is at least one of acetic acid, tartaric acid and citric acid.
[0016] In addition, the present invention also provides a method for preparing the high-efficiency soft-hand wet friction fastness enhancer, comprising the following steps:
[0017] S1, adding the formulated amount of polyether and tristyrylphenol polyoxyethylene ether into a reactor for dehydration treatment;
[0018] S2, cooling the reactor to 50-60°C and adding solvent;
[0019] S3, adding isocyanate polymer, and reacting at a constant temperature for 0.5-1h, then raising the temperature to 70-90°C, and reacting at a constant temperature for 1-4h to obtain a polyurethane prepolymer;
[0020] S4, adding active hydride containing tertiary amino group, and reacting at a constant temperature of 70-90°C for 1-2h;
[0021] S5, adding hydroxy silicone oil for chain extension, and reacting at 70-90°C for 1-2h;
[0022] S6, cool down to 60°C, add deionized water to emulsify evenly, and cool down to room temperature;
[0023] S7, adding a diamine type chain extender, and carrying out a chain extension reaction at 20-40°C for 15min-1h;
[0024] S8, adding acid for neutralization;
[0025] S9, heating and distilling to remove the solvent to obtain a wet friction fastness improving agent with a content of 20-25%.
[0026] The mechanism of the present invention is:
[0027] The present invention adopts an isocyanate polymer, preferably a TDI trimer (DESMODUR L75), which is formed by self-polymerization of TDI and has the performance of TDI. It has three benzene rings in its structure, and its smoothness and wear resistance are better than TDI, which can greatly improve the wear resistance of the polyurethane film. The present invention adopts tristyrylphenol polyoxyethylene ether 16EO, which contains three benzene rings in its structure, and the three benzene rings are in the same plane, which can improve the film-forming property and smoothness of the fabric and improve the friction resistance effect; at the same time, the compound has a surfactant property, and after reacting with the isocyanate polymer, it can improve the stability of the wet friction fastness enhancer. The present invention adopts an active hydrogen containing a tertiary amino group, which contains an amino group. After the amino group is protonated, the polyurethane is cationic, which can make the polyurethane film better combined with the fabric, improve the stability of the polyurethane, and at the same time, the amino group can give the fabric a certain soft feel; adding the double-terminal hydroxy silicone oil can allow the present invention to give the fabric a good soft feel, and there is no problem that the fabric feels hard and rough after using a conventional wet friction fastness enhancer.
[0028] Compared with the prior art, the wet rubbing fastness improver of the present invention can effectively improve the wet rubbing fastness of fabrics and enhance the softness of the fabric feel. Under the same dosage, the wet rubbing fastness improving effect of the fabric is better than that of conventional wet rubbing fastness improvers, and the fabric can be given an excellent feel. Moreover, the raw material safety of the wet rubbing fastness improver of the present invention is better than that of conventional wet rubbing fastness improvers, and the toxicity is low, so the wet rubbing fastness improver is an ideal fabric dyeing and printing auxiliary agent. DETAILED DESCRIPTION
[0029] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention is further described in detail below. However, it should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the scope of the present invention. Unless otherwise defined, all technical terms and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention, and the terms used in the specification of the present invention herein are only for the purpose of describing specific embodiments and are not intended to limit the present invention.
[0030] Example 1
[0031] A method for preparing a high-efficiency soft-touch wet friction fastness enhancer comprises the following steps:
[0032] S1, add 60.0g PEG1000 (polyethylene glycol 1000) and 16.2g tristyrylphenol polyoxyethylene ether 16EO (marketed model Nongru 600#F, available in Zhejiang Huangma) into the reactor, heat to 110°C and vacuum for 1.5h to dehydrate;
[0033] S2, after the vacuum dehydration in step S1 is completed, the vacuum is broken, nitrogen is replaced, the reactor is cooled to 55°C, 76.2g of butanone is added, and stirred evenly;
[0034] S3, slowly dropwise add 90 g of Desmodur L 75 (commercially available, Desmodur L75 Covestro, Germany, Chinese name: aromatic polyisocyanate based on toluene diisocyanate), stir evenly, keep the reaction at 55° C. for 0.5 h, slowly raise the temperature to 75° C., keep the reaction at this temperature for 2 h, and obtain a polyurethane prepolymer;
[0035] S4, add 1.5g N-methyldiethanolamine, and react at 75°C for 1h;
[0036] S5, slowly add 60g of 3000 molecular weight hydroxy silicone oil, and keep the reaction at 75℃ for 1.5h;
[0037] S6, cool to 60°C, add 728.1 g of deionized water under rapid stirring, and cool to 30°C with ice water;
[0038] S7, add 1.5 g of ethylenediamine, and carry out chain extension reaction at 30°C for 1 h;
[0039] S8, adding 1.5g acetic acid for neutralization;
[0040] S9, heating and distilling to remove the solvent, filtering the product, and diluting it to a solid content of 20% to obtain a uniform and stable wet friction fastness improving agent.
[0041] Example 2
[0042] A method for preparing a high-efficiency soft-touch wet friction fastness enhancer comprises the following steps:
[0043] S1, add 40g PEG1000, 10g polytetramethylene ether PTMEG2000, and 20g tristyrylphenol polyoxyethylene ether 16EO into the reactor, heat to 115°C and vacuum for 1.5h to dehydrate;
[0044] S2, after the vacuum dehydration in step S1 is completed, break the vacuum, replace with nitrogen, cool to 55°C, add 70g of butanone, and stir evenly;
[0045] S3, slowly dropwise add 90g of Desmodur L75, stir evenly, keep the mixture at 55°C for 0.5h, slowly raise the temperature to 75°C, keep the mixture for 2h, and obtain a polyurethane prepolymer;
[0046] S4, add 1.5g N-methyldiethanolamine, and keep the reaction at 75℃ for 1h;
[0047] S5, slowly add 50g of 2000 molecular weight hydroxy silicone oil, and keep the reaction at 75℃ for 1.5h;
[0048] S6, cool to 60°C, add 669.5g of deionized water under rapid stirring, and cool to 30°C with ice water;
[0049] S7, add 1.5 g of ethylenediamine dropwise, and react at room temperature of 30°C for 1 hour;
[0050] S8, adding 1.5g acetic acid for neutralization;
[0051] S9, removing the solvent by distillation at elevated temperature, filtering the product, and diluting it to a solid content of 20% to obtain a uniform and stable wet friction fastness enhancer.
[0052] Example 3
[0053] A method for preparing a high-efficiency soft-touch wet friction fastness enhancer comprises the following steps:
[0054] S1, add 25g PEG1000, 25g PEG2000, and 20g tristyrylphenol polyoxyethylene ether 16EO into the reactor, heat to 120°C and vacuum for 1.5h to dehydrate;
[0055] S2, after the vacuum dehydration in step S1 is completed, break the vacuum, replace with nitrogen, cool to 55°C, add 70g of butanone, and stir evenly;
[0056] S3, slowly dropwise add 90g of Desmodur L75, stir evenly, keep the mixture at 60°C for 0.5h, slowly raise the temperature to 80°C, keep the mixture for 2h, and obtain a polyurethane prepolymer;
[0057] S4, add 1.5g N-methyldiethanolamine, and keep the reaction at 80℃ for 1h;
[0058] S5, slowly add 60g of 2000 molecular weight hydroxy silicone oil, and keep the reaction at 80℃ for 1.5h;
[0059] S6, cool to 60°C, add 709.54 g of deionized water under rapid stirring, and cool to 30°C with ice water;
[0060] S7, add 1.5 g of ethylenediamine dropwise, and react at room temperature for 0.5 h;
[0061] S8, adding 1.5g acetic acid for neutralization;
[0062] S9. Remove the solvent by distillation, filter the product, and dilute it to 20% solid content to obtain a uniform and stable wet friction fastness enhancer.
[0063] Comparative Example 1
[0064] Step 1, add 38g PEG1000 and 38g PEG2000 into the reactor, heat to 115°C and vacuum for 1.5h to dehydrate;
[0065] Step 2: After vacuuming, break the vacuum, replace with nitrogen, cool to 55°C, add 76g of butanone, and stir evenly;
[0066] Step 3, slowly drop 20g TDI, stir evenly, keep the temperature at 60°C for 0.5h, slowly heat to 75°C, keep the temperature for 2h, and obtain a polyurethane prepolymer;
[0067] Step 4, add 1.5g N-methyldiethanolamine, and react at 75°C for 1h;
[0068] Step 5, cool to 60°C, add 320g of deionized water under rapid stirring, and cool to 30°C with ice water;
[0069] Step 6, add 1.5 g of ethylenediamine dropwise and react at room temperature for 1 h;
[0070] Step 7, add 1.5g acetic acid to neutralize;
[0071] Step 8: removing the solvent by distillation, filtering the product, and diluting it to a solid content of 20% to obtain a uniform and stable wet friction fastness enhancer.
[0072] Fabric treatment
[0073] Dyeing process: dyeing (8% (owf)) dye solution, 80g / L sodium chloride, 30g / L soda ash, bath ratio 1:20→soaping (2g / L, soaping agent) bath ratio 1:40, 95℃*15min→washing→drying. Finishing process: dyed cloth→padding (20g / L, 50g / L wet friction fastness enhancer, 30℃, one dip and one pad, padding rate: 80%)→170℃*2.5min setting and drying→after cooling, compare the wet friction fastness grade and the feel.
[0074] The finished fabric was tested for performance according to HG / T 5498-2018, and the test results are shown in Table 1 below.
[0075] Table 1 Fabric properties after finishing
[0076] Performance effect / sample Example 1 Example 2 Example 3 Comparative Example 1 20g / L wet friction fastness improver wet friction effect 4.5 5 5 3 20g / L fabric softness rating 4.5 5 5 2 50g / L wet friction fastness improver wet friction effect 5 5 5 3 50g / L fabric softness rating 4.5 5 5 2
[0077] From the analysis of Table 1, it can be seen that the wet rubbing fastness improver of the present invention can effectively improve the wet rubbing fastness of the fabric and enhance the softness of the fabric. Under the same dosage, the effect of improving the wet rubbing fastness of the fabric is better than that of the conventional wet rubbing fastness improver, and the fabric is given an excellent hand feel. Moreover, the raw material safety of the wet rubbing fastness improver of the present invention is better than that of the conventional wet rubbing fastness improver, and the toxicity is low, so the wet rubbing fastness improver of the present invention is an ideal fabric dyeing and printing auxiliary agent.
[0078] The above is only a preferred embodiment of the present invention. It should be pointed out that for those skilled in the art, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as within the scope of protection of the present invention.
Claims
1. A high-efficiency soft-hand wet friction fastness enhancer, characterized in that: The raw materials include, by mass: 40-100 parts of polyether, 10-30 parts of tristyrylphenol polyoxyethylene ether 16EO, 40-100 parts of solvent, 60-120 parts of isocyanate polymer, 0.5-4 parts of active hydride containing tertiary amino group, 40-80 parts of hydroxy silicone oil, 600-800 parts of deionized water, 0.5-3 parts of diamine chain extender, and 0.5-5 parts of acid; The polyether is at least one of PEG1000, PEG2000, and PTMEG2000; the isocyanate polymer is at least one of TDI polymer DESMODUR L75, HDI polymer DESMODUR N100, and HDI polymer DESMODUR N3300; the active hydride containing tertiary amino groups is at least one of N,N-dimethylethanolamine, N-methyldiethanolamine, N,N-dimethylethylenediamine, and triethanolamine; and the diamine chain extender is at least one of ethylenediamine, o-phenylenediamine, hydrazine hydrate, and isophoronediamine.
2. The high-efficiency soft-hand wet friction fastness enhancer according to claim 1, characterized in that: The solvent is at least one of dimethylformamide, tetrahydrofuran, N-methyl-2-pyrrolidone, toluene, propylene glycol monomethyl ether acetate, butanone and acetone.
3. The high-efficiency soft-hand wet friction fastness enhancer according to claim 1, characterized in that: The hydroxy silicone oil is at least one of double-terminal hydroxy silicone oils with a molecular weight of 1000-10000.
4. The high-efficiency soft-hand wet friction fastness enhancer according to claim 1, characterized in that: The acid is at least one of acetic acid, tartaric acid and citric acid.
5. A method for preparing the high-efficiency soft-hand wet friction fastness enhancer according to any one of claims 1 to 4, characterized in that: The following steps are involved: S1, adding the formulated amount of polyether and tristyrylphenol polyoxyethylene ether into a reactor for dehydration treatment; S2, cooling the reactor to 50-60°C and adding solvent; S3, adding isocyanate polymer, and reacting at a constant temperature for 0.5-1h, then raising the temperature to 70-90°C, and reacting at a constant temperature for 1-4h to obtain a polyurethane prepolymer; S4, adding active hydride containing tertiary amino group, and reacting at a constant temperature of 70-90°C for 1-2h; S5, adding hydroxy silicone oil for chain extension, and reacting at 70-90°C for 1-2h; S6, cool down to 60°C, add deionized water to emulsify evenly, and cool down to room temperature; S7, adding a diamine type chain extender, and carrying out a chain extension reaction at 20-40°C for 15min-1h; S8, adding acid for neutralization; S9, heating and distilling to remove the solvent to obtain a wet friction fastness enhancer with a content of 20-25%.
Citation Information
Patent Citations
An environmentally friendly polyether-silicone modified polyurethane and its preparation method
CN106893042B
Lasting wet friction firmness increasing agent and preparation method thereof
CN102432801A
Color fixing agent for cotton fabrics and preparation method thereof
CN109208355A