A high pressure forming method for laminated polycarbonate sheet

The polycarbonate plate and TPU film are processed in curved glass molds through high-pressure molding, which solves the problem that polycarbonate plate cannot be processed on the curved surface, realizes the production of curved laminated polycarbonate plates, and improves its bonding fastness and service life.

CN116198064BActive Publication Date: 2024-11-19QINGDAO ZHONGXINGTONG RAIL TRANSIT TECH CO LTD
View PDF 17 Cites 0 Cited by

Patent Information

Application Number
CN202310183056.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-01
Publication Date
2024-11-19
Estimated Expiration
2043-03-01

AI Technical Summary

Technical Problem

Existing polycarbonate plates cannot be processed in curved surfaces, and the curved laminated polycarbonate plates cannot be produced.

Method used

By adopting the high-pressure molding method, TPU film is laid in the middle of the polycarbonate plate and fixed in the hot-bending curved glass mold, vacuum cooling pumping and high-temperature and high-pressure treatment are carried out, and the curved clamp is formed by using the hot melt bonding strength of the TPU film. Glue polycarbonate board.

Benefits of technology

The curved surface laminated polycarbonate plate was successfully produced, which improved its bonding fastness and service life, avoided bubbles and deformation problems in the finished product, and ensured the uniformity and stability of the curved surface.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004102841130000131
    Figure BDA0004102841130000131
Patent Text Reader

Abstract

The present application relates to the field of production of transparent parts for rail transit, and specifically discloses a high-pressure molding method for a laminated polycarbonate plate, comprising the following steps: S1, heating two glasses to 600-700°C to prepare a curved glass mold; S2, laying a TPU film between the two polycarbonate plates to obtain a laminated part; S3, placing the laminated part between the two curved glass molds, and then fixing it to obtain a fixed part; S4, subjecting the fixed part to a vacuum cold-drawing treatment, and then subjecting the fixed part to a high-temperature and high-pressure treatment at a temperature of 50-135°C and a pressure of 0.05-1.2MPa for 160-260min, and then removing the curved glass mold to obtain a laminated polycarbonate plate; and obtaining a curved laminated polycarbonate plate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of rail transit transparent parts production, and more specifically, to a high-pressure molding method for laminated polycarbonate sheets. Background Art

[0002] In the deep processing enterprises of glass transparent parts for rail transit, with the requirements of lightweight design, polycarbonate sheets are continuously introduced into the use of rail transit transparent parts.

[0003] Polycarbonate board is made of polycarbonate polymer. It is a new type of high-strength, light-transmitting building material. It is the best building material to replace glass and plexiglass. Compared with tempered glass, laminated glass and insulating glass, PC board has the advantages of lighter weight, weather resistance, super strength, flame retardancy and sound insulation.

[0004] However, due to the characteristics of the existing polycarbonate sheets, only flat sheets can be produced and curved surface processing cannot be performed, so it is impossible to produce polycarbonate sheets with curved surfaces.

[0005] Therefore, how to produce a curved laminated polycarbonate sheet is a problem to be solved. Summary of the invention

[0006] In order to produce a laminated polycarbonate sheet with a curved surface, the present application provides a high-pressure forming method for a laminated polycarbonate sheet.

[0007] The present application provides a high pressure forming method for a laminated polycarbonate sheet, which adopts the following technical solution:

[0008] A high pressure forming method for a laminated polycarbonate sheet comprises the following steps:

[0009] S1, heating two glasses to 600-700° C. to prepare a curved glass mold;

[0010] S2, laying a TPU film between two polycarbonate plates to obtain a laminated part;

[0011] S3, placing the laminated part between two curved glass molds, and then fixing it to obtain a fixed part;

[0012] S4. The fixing parts are subjected to vacuum cold extraction treatment, and then subjected to high temperature and high pressure treatment for 160-260 min at a temperature of 50-135° C. and a pressure of 0.05-1.2 MPa, and then the curved glass mold is removed to obtain a laminated polycarbonate board.

[0013] By adopting the above technical scheme, two glasses are softened and hot-bent at 600-700°C to obtain a curved glass mold. After the laminated parts are placed in the two curved glass molds, they are vacuum-cooled to remove residual air in the structure, thereby avoiding bubbles in the finished product as much as possible to affect the quality of the curved finished product. Then, under high temperature and high pressure treatment conditions, the polycarbonate sheet is gradually deformed, and the TPU film is gradually melted. The higher bonding strength of the TPU film after hot melting is used to bond the two curved polycarbonate sheets to obtain a curved laminated polycarbonate sheet.

[0014] Preferably, the vacuum pressure of the vacuum cold pumping treatment in S4 is -0.08 to -0.1 MPa, and the time is 4 to 8 hours.

[0015] By adopting the above technical solution, it is ensured that there is no air between the two polycarbonate sheets, thereby ensuring that the finished laminated polycarbonate sheet has good bonding strength and a long service life.

[0016] Preferably, the specific steps of high temperature and high pressure treatment in S4 are as follows:

[0017] Raise the temperature to 50-60℃ while introducing air at a pressure of 0.05-0.15MPa, maintain for 50-90min, then raise the temperature to 90-100℃, maintain for 50-90min at a pressure of 0.1-0.2MPa, finally raise the temperature to 125-135℃, maintain for 60-80min at a pressure of 1.1-1.2MPa; then keep the pressure unchanged, cool to below 50℃, and exhaust to normal pressure.

[0018] By adopting the above technical solution, in the first stage, the polycarbonate sheet is kept warm at 50-60℃ and 0.05-0.15MPa, so that the polycarbonate sheet is deformed by force. During the bending process of the polycarbonate sheet, the TPU film is also gradually bent. At this time, the TPU film is not hot-melted, but the overall temperature of the TPU film is maintained at 50-60℃, so as to ensure that the TPU film is in uniform contact with the polycarbonate sheet. If the TPU film is hot-melted at the beginning of bending, it will not only easily affect the realization of subsequent bending, but also the bending surface of the subsequent bending will not be easy to evenly adhere to the glue of the TPU film, which will not only easily generate bubbles and hollows, but more importantly, affect the strength, shape and stability of the laminated polycarbonate sheet.

[0019] By limiting the heat preservation time of the first stage, it is ensured that the polycarbonate completes the deformation under the physical pressure of the curved glass mold.

[0020] In the second stage, the temperature is raised to 90-100°C and the pressure is 0.1-0.2MPa, so that the TPU film gradually softens and melts to produce viscosity, so as to facilitate the bonding of the two polycarbonate plates after the deformation is completed. By limiting the insulation time, it is ensured that the TPU film is evenly heated and the two polycarbonate plates are evenly bonded, which makes it less likely to have problems such as good bonding stability in some parts and poor bonding stability in others.

[0021] In the third stage, the temperature is raised to 125-135°C and the pressure is 1.1-1.2MPa, so that the polycarbonate sheet is gradually softened and stabilized, and the TPU film is completely hot-melt and the viscosity basically reaches the peak value. The hot-melt TPU film stably and evenly bonds the two polycarbonate sheets, thereby improving the bonding strength and bonding stability of the laminated polycarbonate sheet; and the physical deformation in the early stage is combined with the chemical softening deformation in the later stage to ensure that the bending stability of the finished laminated polycarbonate sheet is good, so that the laminated polycarbonate sheet is not prone to the problem of straightening deformation.

[0022] If a single physical deformation occurs, the polycarbonate sheet will easily rebound during use, and if a single softening deformation occurs, it will easily affect the bonding uniformity of the TPU film, thereby affecting the bonding strength of the TPU film. Therefore, by adopting different temperature, pressure, and insulation time limits at different stages, the two polycarbonate sheets in the finished laminated polycarbonate sheet have the advantages of high bonding strength and good bonding stability, and the laminated polycarbonate sheet is not easy to deform and rebound.

[0023] Preferably, the polycarbonate plate is prepared by the following method:

[0024] Polyvinyl alcohol liquid is evenly sprayed on the surface of a commercially available polycarbonate plate at a mass ratio of 1:0.02-0.06, and then water-white rosin resin particles are evenly sprayed. The mass ratio of the commercially available polycarbonate plate to the water-white rosin resin particles is 1:0.1-0.22. After drying, a finished product is obtained.

[0025] By adopting the above technical solution, polyvinyl alcohol liquid and water-white rosin resin particles are matched, and the viscosity of the polyvinyl alcohol liquid is utilized to make the water-white rosin resin particles adhere to the surface of the commercially available polycarbonate plate.

[0026] When the polycarbonate sheet is treated with high temperature and high pressure, under the condition of 120-135°C, the water-white rosin resin on the surface of the polycarbonate softens but does not melt. After the TPU film is melted, the hot-melt thermoplastic polyurethane elastomer is bound by the bonding and cross-linking effect of the amino group in the thermoplastic polyurethane elastomer, the carboxyl group in the water-white rosin resin and the hydroxyl group in the polyvinyl alcohol, so as to avoid the hot-melt TPU film from flowing between the two polycarbonate sheets as much as possible, thereby affecting the bonding flatness and uniformity between the two polycarbonate sheets. In addition, at the curved surface, due to the increase in slope, it is easier for the hot-melt TPU film to flow, so that it is more likely to have less glue at the vertex of the curved surface and more glue at other positions. The combination of thermoplastic polyurethane elastomer, polyvinyl alcohol liquid and water-white rosin resin particles makes the two polycarbonate sheets in the laminated polycarbonate sheet have the advantages of high bonding strength, good bonding stability and uniform bonding, thereby improving the quality and service life of the laminated polycarbonate sheet.

[0027] The TPU film, polyvinyl alcohol liquid and water-white rosin resin particles are matched, and the bonding and cross-linking effect of the TPU film, polyvinyl alcohol and water-white rosin resin is utilized to further improve the bonding stability between the TPU film and the two polycarbonate sheets, so that the finished laminated polycarbonate sheet is not prone to the problem of the bent parts straightening during long-term use, and the finished laminated polycarbonate sheet has a longer service life and stability in use.

[0028] Preferably, the TPU film is prepared by the following method:

[0029] Weigh 60-90 parts of thermoplastic polyurethane elastomer, 1-5 parts of coated PMMA particles, and 1-5 parts of polyacrylamide-modified transparent mica sheets, mix and stir evenly, and perform molding treatment to obtain a TPU film.

[0030] By adopting the above technical scheme, thermoplastic polyurethane elastomer, coated PMMA particles, polyacrylamide-modified transparent mica sheets, polyvinyl alcohol, and water-white rosin resin particles are matched, and the water-white rosin resin and polyvinyl alcohol on the surface of the polycarbonate board are used to stabilize the hot-melt TPU film, so that the TPU film is not easy to flow after hot melting, ensuring that the two polycarbonate boards in the laminated polycarbonate board have good bonding stability and bonding uniformity, thereby improving the quality and service life of the laminated polycarbonate board.

[0031] By utilizing the compatible bonding effect of the amide group in polyacrylamide and the amino group in thermoplastic polyurethane elastomer, the transparent mica sheet is more stably bonded to the inside of the TPU film, while the PMMA particles have good dispersibility and can be evenly dispersed inside the TPU film, and have good bonding stability with the thermoplastic polyurethane elastomer.

[0032] During the preparation of the laminated polycarbonate board, as the temperature rises, the thermoplastic polyurethane elastomer gradually melts and flows, but the coated PMMA particles and polyacrylamide-modified transparent mica sheets do not melt and are not easy to flow, thereby stabilizing the thermoplastic polyurethane elastomer and making the gradually melting thermoplastic polyurethane elastomer not easy to flow.

[0033] At the same time, the hydroxyl groups on the polyvinyl alcohol on the surface of the polycarbonate board and the carboxyl groups in the water-white rosin resin are attracted to the amino groups in the hot-melt thermoplastic polyurethane elastomer and the amide groups in the polyacrylamide. The softening but non-flowing effect of the water-white rosin resin is used to stabilize the polyamide-modified transparent mica sheets, coated PMMA particles and thermoplastic polyurethane elastomer, so that the hot-melt thermoplastic polyurethane elastomer is not easy to flow, ensuring that the two polycarbonate boards in the laminated polycarbonate board have good bonding stability and bonding uniformity.

[0034] Thermoplastic polyurethane elastomer, coated PMMA particles, and polyacrylamide modified transparent mica sheets are combined, and the good transparency and weather resistance of PMMA particles and transparent mica sheets are utilized to ensure that the finished laminated polycarbonate has good transparency and a long service life.

[0035] Preferably, the coated PMMA particles are prepared by the following method:

[0036] Weighing PMMA particles, etching them, and then dispersing and soaking them in a 0.1-0.5% sodium carboxymethyl cellulose solution, taking them out and drying them to obtain loaded PMMA particles;

[0037] The EVA particles are immersed and dispersed in a sodium carboxymethyl cellulose aqueous solution having a concentration of 0.5-1%, and then the EVA particles are taken out to obtain loaded EVA particles;

[0038] The loaded EVA particles are uniformly sprayed on the surface of the loaded PMMA particles at a mass ratio of 1:1-2, and the finished product is obtained after drying.

[0039] By adopting the above technical scheme, PMMA particles are etched, soaked in sodium carboxymethyl cellulose solution, and coated with EVA particles, and the large number of gap structures on the surface of PMMA particles are utilized to increase the contact area between PMMA particles and thermoplastic polyurethane elastomers. In combination with the good bonding compatibility of EVA particles with thermoplastic polyurethane elastomers and polyacrylamide, the thermoplastic polyurethane elastomer is not easy to flow after hot melting, thereby ensuring the bonding stability of the TPU film between the two polycarbonate plates.

[0040] After the PMMA particles are etched, there are gap structures on the surface of the PMMA particles. Then, the PMMA particles are immersed in a low concentration of sodium carboxymethyl cellulose solution, so that the sodium carboxymethyl cellulose adheres to the surface of the PMMA particles while not making it easy for the PMMA particles to bond and agglomerate. In addition, sodium carboxymethyl cellulose is also attached to the surface of the EVA particles. When the loaded PMMA particles are coated with the loaded EVA particles, carboxyl groups are attached to the surface of the prepared coated PMMA particles. The carboxyl groups in sodium carboxymethyl cellulose, the amino groups in the thermoplastic polyurethane elastomer, and the amide groups in the polyacrylamide are used to further improve the adhesion between the coated PMMA particles and the thermoplastic polyurethane elastomer and the polyacrylamide-modified transparent cloud. The bonding stability between the mother sheets is further prevented, thereby further preventing the thermoplastic polyurethane elastomer from gradually flowing after hot melting, so that the TPU film has better bonding uniformity; at the same time, at a temperature of 120-135°C, EVA particles are easy to gradually melt, and the hot-melted EVA has higher viscosity. EVA and thermoplastic polyurethane elastomer have good bonding compatibility, and the gap structure on the surface of PMMA particles is combined to further stabilize the hot-melt thermoplastic polyurethane elastomer, making it difficult for the thermoplastic polyurethane elastomer in the TPU film to flow, thereby ensuring the bonding uniformity and bonding stability of the TPU film between the two polycarbonate sheets, so as to extend the service life of the laminated polycarbonate sheet.

[0041] PMMA particles, EVA particles and thermoplastic polyurethane elastomer are matched, and the high elastic structure of EVA particles and thermoplastic polyurethane elastomer is utilized to make an elastic buffer structure exist on the surface of PMMA particles. When the laminated polycarbonate board is in the preparation process, even after high pressure treatment, PMMA particles are not easy to affect the polycarbonate board, thereby ensuring that the laminated polycarbonate board has high quality and long service life.

[0042] Preferably, PET high temperature tape is used for fixing in S3.

[0043] By adopting the above technical solution, the PET high temperature tape is used to fix the laminated parts, so that the laminated parts are not prone to structural changes when being treated with high temperature and high pressure, thereby ensuring the processing quality of the finished laminated polycarbonate board; and the PET high temperature tape has good high temperature resistance, and is not prone to changes in physical and chemical properties even when treated under high temperature and high pressure conditions; at the same time, the PET high temperature tape is easy to tear off and is not prone to leaving residues on the surface of the finished laminated polycarbonate.

[0044] Preferably, the PET high temperature tape is prepared by the following method:

[0045] The adhesive is sprayed evenly on the PET substrate and rolled to obtain a finished product; the adhesive is composed of organic silicone adhesive and polyamide resin particles in a mass ratio of 1:0.05-0.2.

[0046] By adopting the above technical scheme, the organic silicone adhesive and the polyamide resin particles are matched. When the thermoplastic polyurethane elastomer in the TPU film melts and flows to extrude the PET high-temperature tape, the elasticity of the polyamide resin particles can buffer the extrusion of the PET high-temperature tape by the flowing TPU film, and the hot-melt thermoplastic polyurethane elastomer in the TPU film flows out of the polycarbonate plate surface to produce bulges, so that the PET high-temperature tape is stably attached to the surface of the sandwich component and is not prone to detachment.

[0047] The mass ratio of the organic silicone adhesive and the polyamide resin particles is limited so that the polyamide resin particles are dispersed in the internal structure of the organic silicone adhesive, so that the polyamide resin particles do not directly contact the TPU film, thereby making it difficult for the TPU film to contact the polyamide resin particles, thereby improving the bonding strength, making it easy for the PET high-temperature tape to be torn off the laminated polycarbonate surface, and not easy for the adhesive to leave residue.

[0048] Preferably, a TPU isolation film is provided between the laminated component and the two curved glass molds in S3.

[0049] By adopting the above technical solution and utilizing the good isolation and protection effect of the TPU isolation film, the surfaces of the two polycarbonate plates are protected from being scratched by the two curved glass molds, thereby ensuring that the finished laminated polycarbonate plate has good quality and a long service life.

[0050] Preferably, the TPU isolation film is prepared by the following method:

[0051] Thermoplastic polyurethane elastomer and aluminum oxide powder are weighed and mixed in a mass ratio of 1:0.02-0.06, and stirred evenly, and molded to obtain a finished product.

[0052] By adopting the above technical scheme, thermoplastic polyurethane elastomer and alumina powder are matched, and the good thermal conductivity of alumina is utilized, combined with the good elasticity of thermoplastic polyurethane elastomer, so that the TPU isolation film can conduct heat evenly and quickly, while utilizing elastic buffering to protect the polycarbonate plate from being scratched by the glass mold, thereby ensuring that the finished laminated polycarbonate plate has good quality and a long service life.

[0053] In summary, this application has the following beneficial effects:

[0054] 1. After the laminated parts are placed in two curved glass molds, they are vacuum-drawn to remove the remaining air in the structure, so as to avoid bubbles in the finished product and affect the quality of the curved finished product; then, under high temperature and high pressure treatment conditions, the polycarbonate sheet gradually deforms, and the TPU film gradually melts. The high bonding strength of the TPU film after hot melting is used to bond the two curved polycarbonate sheets together to obtain a curved laminated polycarbonate sheet.

[0055] 2. By adopting different temperature, pressure and insulation time limits at different stages, the two polycarbonate sheets in the finished laminated polycarbonate sheet have the advantages of high bonding strength and good bonding stability, and the laminated polycarbonate sheet is not prone to deformation and rebound.

[0056] 3. TPU film, polyvinyl alcohol liquid and water-white rosin resin particles are matched, and the bonding and cross-linking effect of TPU film, polyvinyl alcohol and water-white rosin resin is utilized to further improve the bonding stability between TPU film and two polycarbonate sheets, so that the finished laminated polycarbonate sheet is not prone to the problem of straightening the bent parts during long-term use, so that the finished laminated polycarbonate sheet has a longer service life and stability in use. DETAILED DESCRIPTION

[0057] The present application is further described in detail below with reference to the embodiments.

[0058] Preparation Example of Polycarbonate Plate

[0059] The polycarbonate sheet in the following raw materials was purchased from Sabic Corporation, model HLG5; the water-white rosin resin particles were purchased from Jinan Jinyu Chemical Co., Ltd.

[0060] Preparation Example 1: A polycarbonate plate is prepared by the following method:

[0061] 0.05 kg of polyvinyl alcohol liquid was evenly sprayed on the surface of 1 kg of commercially available polycarbonate board. The polyvinyl alcohol liquid was a 10% polyvinyl alcohol aqueous solution. Then 0.2 kg of water-white rosin resin particles were evenly sprayed. The particle size of the water-white rosin resin particles was 20 μm. After drying, a finished product was obtained.

[0062] Preparation Example 2: A polycarbonate plate is prepared by the following method:

[0063] 0.02 kg of polyvinyl alcohol liquid was evenly sprayed on the surface of 1 kg of commercially available polycarbonate board. The polyvinyl alcohol liquid was a 10% polyvinyl alcohol aqueous solution. Then 0.1 kg of water-white rosin resin particles were evenly sprayed. The particle size of the water-white rosin resin particles was 20 μm. After drying, a finished product was obtained.

[0064] Preparation Example 3: A polycarbonate plate is prepared by the following method:

[0065] 0.06 kg of polyvinyl alcohol liquid was evenly sprayed on the surface of 1 kg of commercially available polycarbonate plate. The polyvinyl alcohol liquid was a 10% polyvinyl alcohol aqueous solution. Then 0.22 kg of water-white rosin resin particles were evenly sprayed. The particle size of the water-white rosin resin particles was 20 μm. After drying, a finished product was obtained.

[0066] Preparation example of coated PMMA particles

[0067] Preparation Example 4: Coated PMMA particles were prepared by the following method:

[0068] Weigh PMMA particles and process them through laser etching, wherein the depth of the cracks on the surface of the PMMA particles is 5 μm and the width is 1 μm, and the particle size of the PMMA microspheres is 20 μm, and then place them in a 0.3% sodium carboxymethyl cellulose solution for dispersion and immersion, wherein the sodium carboxymethyl cellulose solution is a sodium carboxymethyl cellulose aqueous solution, take out the PMMA particles and dry them, and obtain loaded PMMA particles; place EVA particles in a 1% sodium carboxymethyl cellulose aqueous solution for immersion and dispersion, and then take out the EVA particles, wherein the melting point of the EVA particles is 95° C. and the particle size of the EVA particles is 5 μm, and obtain loaded EVA particles;

[0069] 1.5 kg of loaded EVA particles were uniformly sprayed on the surface of 1 kg of loaded PMMA particles, and the finished product was obtained after drying, and the particle size of the finished product was less than 40 μm.

[0070] Preparation Example 5: Coated PMMA particles were prepared by the following method:

[0071] Weigh PMMA particles and process them through laser etching, wherein the depth of the cracks on the surface of the PMMA particles is 5 μm and the width is 1 μm, and the particle size of the PMMA microspheres is 20 μm, and then place them in a 0.1% sodium carboxymethyl cellulose solution for dispersion and immersion, wherein the sodium carboxymethyl cellulose solution is a sodium carboxymethyl cellulose aqueous solution, take out the PMMA particles and dry them to obtain loaded PMMA particles; place EVA particles in a 0.5% sodium carboxymethyl cellulose aqueous solution for immersion and dispersion, and then take out the EVA particles, wherein the melting point of the EVA particles is 95° C. and the particle size of the EVA particles is 5 μm, to obtain loaded EVA particles;

[0072] 1 kg of loaded EVA particles were uniformly sprayed on the surface of 1 kg of loaded PMMA particles, and the finished product was obtained after drying. The particle size of the finished product was 30 μm.

[0073] Preparation Example 6: Coated PMMA particles were prepared by the following method:

[0074] Weigh PMMA particles and process them with laser etching, wherein the depth of the cracks on the surface of the PMMA particles is 5 μm and the width is 1 μm, and the particle size of the PMMA microspheres is 20 μm, and then place them in a 0.5% sodium carboxymethyl cellulose solution for dispersion and immersion, wherein the sodium carboxymethyl cellulose solution is a sodium carboxymethyl cellulose aqueous solution, take out the PMMA particles and dry them to obtain loaded PMMA particles; place EVA particles in a 1% sodium carboxymethyl cellulose aqueous solution for immersion and dispersion, and then take out the EVA particles, wherein the melting point of the EVA particles is 90° C. and the particle size of the EVA particles is 5 μm, to obtain loaded EVA particles;

[0075] 2kg of loaded EVA particles were uniformly sprayed on the surface of 1kg of loaded PMMA particles, and the finished product was obtained after drying. The particle size of the finished product was 30μm.

[0076] Preparation example of polyacrylamide modified transparent mica flakes

[0077] The transparent mica sheets in the following raw materials were purchased from Lingshou County Ningbo Mineral Products Co., Ltd.; other raw materials and equipment were all commercially available.

[0078] Preparation Example 7: Polyacrylamide modified transparent mica flakes are prepared by the following method:

[0079] 0.3 kg of 1% sodium carboxymethyl cellulose aqueous solution was uniformly sprayed on the surface of 1 kg of transparent mica sheets, the particle size of the transparent mica sheets was 40 μm, and then polyacrylamide particles were uniformly sprayed, the particle size of the polyacrylamide particles was 10 μm, and after drying, a finished polyacrylamide modified transparent mica sheet was obtained, and the finished product particle size was less than 80 μm.

[0080] Preparation example of TPU film

[0081] Thermoplastic polyurethane elastomer in the following raw materials was purchased from Suzhou Yuchenlong Engineering Plastics Co., Ltd., with a melting point of 90°C.

[0082] Preparation Example 8: TPU film is prepared by the following method:

[0083] 80 kg of thermoplastic polyurethane elastomer, 3 kg of coated PMMA particles prepared in Preparation Example 4, and 3 kg of polyacrylamide-modified transparent mica sheets prepared in Preparation Example 7 were weighed and mixed evenly, and melt-extruded and sheeted to obtain a finished TPU film with a thickness of 0.5 mm.

[0084] Preparation Example 9: TPU film is prepared by the following method:

[0085] 60 kg of thermoplastic polyurethane elastomer, 1 kg of coated PMMA particles prepared in Preparation Example 5, and 1 kg of polyacrylamide-modified transparent mica sheets prepared in Preparation Example 7 were weighed and mixed evenly, and melt-extruded and sheeted to obtain a finished TPU film with a thickness of 0.5 mm.

[0086] Preparation Example 10: TPU film is prepared by the following method:

[0087] 90 kg of thermoplastic polyurethane elastomer, 5 kg of coated PMMA particles prepared in Preparation Example 6, and 5 kg of polyacrylamide-modified transparent mica sheets prepared in Preparation Example 7 were weighed and mixed evenly, and melt-extruded and sheeted to obtain a finished TPU film with a thickness of 0.5 mm.

[0088] Preparation example of PET high temperature tape

[0089] The organic silicone adhesive among the following raw materials was purchased from Hubei Longsheng Sihai New Materials Co., Ltd.; other raw materials and equipment were all commercially available.

[0090] Preparation Example 11: PET high temperature tape is prepared by the following method:

[0091] Weigh 1 kg of organic silicone adhesive and 0.1 kg of polyamide resin particles, mix and stir evenly, the particle size of the polyamide resin particles is 100 mesh, to prepare an adhesive;

[0092] The adhesive is evenly sprayed on one side of the PET substrate, the PET substrate is a PET plastic film with a thickness of 1 mm, and the adhesive has a thickness of 0.2 mm, and then rolled to obtain a finished product.

[0093] Preparation Example 12: PET high temperature tape is prepared by the following method:

[0094] Weigh 1 kg of organic silicone adhesive and 0.05 kg of polyamide resin particles, mix and stir evenly, the particle size of the polyamide resin particles is 100 mesh, to prepare an adhesive;

[0095] The adhesive is evenly sprayed on one side of the PET substrate, the PET substrate is a PET plastic film with a thickness of 1 mm, and the adhesive has a thickness of 0.2 mm, and then rolled to obtain a finished product.

[0096] Preparation Example 13: PET high temperature tape is prepared by the following method:

[0097] Weigh 1 kg of organic silicone adhesive and 0.2 kg of polyamide resin particles, mix and stir evenly, the particle size of the polyamide resin particles is 100 mesh, to prepare an adhesive;

[0098] The adhesive is evenly sprayed on one side of the PET substrate, the PET substrate is a PET plastic film with a thickness of 1 mm, and the adhesive has a thickness of 0.2 mm, and then rolled to obtain a finished product.

[0099] Preparation example of TPU isolation film

[0100] Thermoplastic polyurethane elastomer in the following raw materials was purchased from Suzhou Yuchenlong Engineering Plastics Co., Ltd., with a melting point of 150°C.

[0101] Preparation Example 14: TPU isolation film tape is prepared by the following method:

[0102] 1 kg of thermoplastic polyurethane elastomer and 0.04 kg of aluminum oxide powder were weighed and mixed evenly, the particle size of the aluminum oxide powder was 200 nm, and hot-melt extrusion was performed to obtain a finished TPU isolation film with a thickness of 0.2 mm.

[0103] Preparation Example 15: TPU isolation film tape is prepared by the following method:

[0104] 1 kg of thermoplastic polyurethane elastomer and 0.02 kg of aluminum oxide powder were weighed and mixed evenly, the particle size of the aluminum oxide powder was 200 nm, and hot-melt extrusion was performed to obtain a finished TPU isolation film with a thickness of 0.2 mm.

[0105] Preparation Example 16: TPU isolation film tape is prepared by the following method:

[0106] 1 kg of thermoplastic polyurethane elastomer and 0.06 kg of aluminum oxide powder were weighed and mixed evenly, the particle size of the aluminum oxide powder was 200 nm, and hot-melt extrusion was performed to obtain a finished TPU isolation film with a thickness of 0.2 mm.

[0107] Example

[0108] Example 1: A high pressure forming method for laminated polycarbonate sheets:

[0109] S1. Use a hot bending bus furnace to heat two pieces of glass to 650°C. The glass thickness is 8mm. The two pieces of glass are softened and hot bent to obtain a curved glass mold.

[0110] S2, laying a TPU film between two polycarbonate plates to produce a laminate, wherein the polycarbonate plate is the polycarbonate plate prepared in Preparation Example 1, and the TPU film is the TPU film prepared in Preparation Example 8, to obtain a laminated part;

[0111] S3, placing the laminated part between two curved glass molds, laying the TPU isolation film prepared in Preparation Example 14 between the polycarbonate plate and the curved glass mold, and then fixing them with the PET high-temperature tape prepared in Preparation Example 11, and wrapping the PET high-temperature tape around the laminated part and the two curved glasses to obtain a fixing part;

[0112] S4. The fixing parts are subjected to vacuum cold extraction treatment under the action of vacuum pressure of -0.1MPa for a treatment time of 6h, and then subjected to high temperature and high pressure treatment. The temperature is first raised to 55°C while air is introduced at a pressure of 0.1MPa, and maintained for 70min. The temperature is then raised to 95°C and maintained for 70min at a pressure of 0.15MPa. The temperature is finally raised to 135°C and maintained for 70min at a pressure of 1.2MPa. The pressure is then kept unchanged, cooled to 30°C, exhausted to normal pressure, and then the curved glass mold is removed, and the PET high-temperature tape is torn off to obtain a curved polycarbonate plate.

[0113] Example 2: A high pressure forming method for laminated polycarbonate sheets:

[0114] S1. Use a hot bending bus furnace to heat two pieces of glass to 600°C. The glass thickness is 6mm. The two pieces of glass are softened and hot bent to form a curved glass mold.

[0115] S2, laying a TPU film between two polycarbonate plates to produce a laminate, wherein the polycarbonate plate is the polycarbonate plate prepared in Preparation Example 2, and the TPU film is the TPU film prepared in Preparation Example 9, to obtain a laminated part;

[0116] S3, placing the laminated part between two curved glass molds, laying the TPU isolation film prepared in Preparation Example 15 between the polycarbonate plate and the curved glass mold, and then fixing them with the PET high-temperature tape prepared in Preparation Example 12, and wrapping the PET high-temperature tape around the laminated part and the two curved glasses to obtain a fixing part;

[0117] S4. The fixing parts are subjected to vacuum cold extraction treatment under the action of vacuum pressure of -0.08MPa for 4h, and then subjected to high temperature and high pressure treatment. The temperature is first raised to 50°C while air is introduced at a pressure of 0.05MPa, and maintained for 90min. The temperature is then raised to 90°C and maintained for 90min at a pressure of 0.1MPa. The temperature is finally raised to 125°C and maintained for 80min at a pressure of 1.1MPa. The pressure is then kept unchanged, cooled to 40°C, exhausted to normal pressure, and then the curved glass mold is removed, and the PET high temperature tape is torn off to obtain a curved polycarbonate plate.

[0118] Example 3: A high pressure forming method for laminated polycarbonate sheets:

[0119] S1. Use a hot bending bus furnace to heat two pieces of glass to 700°C. The glass thickness is 8mm. The two pieces of glass are softened and hot bent to obtain a curved glass mold.

[0120] S2, laying a TPU film between two polycarbonate plates to produce a laminate, wherein the polycarbonate plate is the polycarbonate plate prepared in Preparation Example 3, and the TPU film is the TPU film prepared in Preparation Example 10, to obtain a laminated part;

[0121] S3, placing the laminated part between two curved glass molds, laying the TPU isolation film prepared in Preparation Example 16 between the polycarbonate plate and the curved glass mold, and then fixing them with the PET high-temperature tape prepared in Preparation Example 13, and wrapping the PET high-temperature tape around the laminated part and the two curved glasses to obtain a fixing part;

[0122] S4. The fixing parts are subjected to vacuum cold extraction treatment under the action of vacuum pressure of -0.1MPa for 8h, and then subjected to high temperature and high pressure treatment. The temperature is first raised to 60°C while air is introduced at a pressure of 0.15MPa, and maintained for 50min. The temperature is then raised to 100°C and maintained for 50min at a pressure of 0.2MPa. The temperature is finally raised to 135°C and maintained for 60min at a pressure of 1.2MPa. The pressure is then kept unchanged, cooled to 50°C, exhausted to normal pressure, and then the curved glass mold is removed, and the PET high temperature tape is torn off to obtain a curved polycarbonate plate.

[0123] Embodiment 4: This embodiment differs from Embodiment 1 in that:

[0124] S4. The fixing parts are subjected to vacuum cold extraction treatment under the action of vacuum pressure of -0.1MPa for a treatment time of 6h, and then subjected to high temperature and high pressure treatment. The temperature is first raised to 55°C while air is introduced at a pressure of 0.1MPa, and maintained for 70min. The temperature is then raised to 75°C and maintained for 70min at a pressure of 0.15MPa. The temperature is finally raised to 135°C and maintained for 70min at a pressure of 1.2MPa. The pressure is then kept unchanged, cooled to 30°C, exhausted to normal pressure, and then the curved glass mold is removed, and the PET high-temperature tape is torn off to obtain a curved polycarbonate plate.

[0125] Embodiment 5: This embodiment differs from Embodiment 1 in that:

[0126] S4. The fixing parts are subjected to vacuum cold extraction treatment under the action of vacuum pressure of -0.1MPa for 6h, and then subjected to high temperature and high pressure treatment. The temperature is first raised to 90°C and maintained for 140min under the pressure of 0.15MPa, and finally raised to 135°C and maintained for 70min under the pressure of 1.2MPa; then the pressure is kept unchanged, cooled to 30°C, vented to normal pressure, and then the curved glass mold is removed, and the PET high temperature tape is torn off to obtain a curved polycarbonate plate.

[0127] Embodiment 6: This embodiment differs from Embodiment 1 in that:

[0128] There is no polyvinyl alcohol liquid and water-white rosin resin particles on the surface of the polycarbonate plate; the coated PMMA particles and polyacrylamide-modified transparent mica sheets are replaced with thermoplastic polyurethane elastomers of equal quality in the raw materials of the TPU film.

[0129] Embodiment 7: This embodiment differs from Embodiment 1 in that:

[0130] No water-white rosin resin particles are added to the polycarbonate board raw materials.

[0131] Embodiment 8: This embodiment differs from Embodiment 1 in that:

[0132] The water-white rosin resin particles in the polycarbonate board raw materials are replaced by EVA particles of equal mass.

[0133] Embodiment 9: This embodiment differs from Embodiment 1 in that:

[0134] The polyvinyl alcohol solution in the polycarbonate board raw material is replaced by an ethyl cellulose ethanol solution of equal mass, wherein the ethyl cellulose ethanol solution has a concentration of 1% and an ethanol solubility of 99%.

[0135] Embodiment 10: This embodiment differs from Embodiment 1 in that:

[0136] In the raw materials of TPU film, the coated PMMA particles and polyacrylamide-modified transparent mica sheets are replaced with silicon dioxide of equal mass.

[0137] Embodiment 11: This embodiment differs from Embodiment 1 in that:

[0138] During the preparation of coated PMMA particles in TPU film, the sodium carboxymethyl cellulose solution is replaced by an ethyl cellulose ethanol solution of equal mass, wherein the ethyl cellulose ethanol solution is a 1% ethyl cellulose ethanol solution and the ethanol solubility is 99%.

[0139] Embodiment 12: This embodiment differs from Embodiment 1 in that:

[0140] No EVA particles were added during the preparation of the coated PMMA particles in the TPU film; the details are as follows:

[0141] Weigh PMMA particles and process them by laser etching. The depth of the cracks on the surface of the PMMA particles is 5 μm and the width is 1 μm. The particle size of the PMMA microspheres is 20 μm. Then, the particles are dispersed and immersed in a 0.3% sodium carboxymethyl cellulose solution. The sodium carboxymethyl cellulose solution is a sodium carboxymethyl cellulose aqueous solution. After taking out the PMMA particles, they are dried to obtain coated PMMA particles.

[0142] Embodiment 13: This embodiment differs from Embodiment 1 in that:

[0143] During the preparation of the coated PMMA particles in the TPU film, the PMMA particles were not etched or immersed in a sodium carboxymethyl cellulose solution for dispersion; the details are as follows:

[0144] 1.5 kg of loaded EVA particles were uniformly sprayed on the surface of 1 kg of PMMA particles, and the finished product was obtained after drying. The particle size of the finished product was less than 40 μm.

[0145] Embodiment 14: This embodiment differs from Embodiment 1 in that:

[0146] In TPU film, the modified transparent mica sheets of the same quality are used to replace the polyacrylamide modified transparent mica sheets.

[0147] The modified transparent mica flakes are prepared as follows:

[0148] 0.3 kg of 1% sodium carboxymethyl cellulose aqueous solution was uniformly sprayed on the surface of 1 kg of transparent mica sheets, the particle size of the transparent mica sheets was 40 μm, and the finished modified transparent mica sheets were obtained after drying.

[0149] Embodiment 15: This embodiment differs from Embodiment 1 in that:

[0150] In TPU film, the modified transparent mica sheets of the same quality are used to replace the polyacrylamide modified transparent mica sheets.

[0151] The modified transparent mica flakes are prepared as follows:

[0152] 0.3 kg of 1% ethyl cellulose ethanol solution was evenly sprayed on the surface of 1 kg of transparent mica sheets, the concentration of ethanol was 99%, and the particle size of the transparent mica sheets was 40 μm. After drying, a finished modified transparent mica sheet was obtained.

[0153] Embodiment 16: This embodiment differs from Embodiment 1 in that:

[0154] During the preparation of the PET high temperature tape, no polyamide resin particles were added to the silicone adhesive raw material.

[0155] Embodiment 17: This embodiment differs from Embodiment 1 in that:

[0156] No alumina powder is added to the TPU isolation film.

[0157] Embodiment 18: This embodiment differs from Embodiment 1 in that:

[0158] No TPU isolation film was added to S3.

[0159] Performance testing

[0160] 1. Uniformity detection

[0161] Finished laminated polycarbonate panels were prepared using the preparation methods of Examples 1-3 and 5-17, respectively. Each square meter of polycarbonate panel was divided into 100 modules of equal size, and the thickness of the modules was measured respectively. The thickness difference = maximum thickness - minimum thickness was recorded, and the data was recorded. The number of bubbles on the surface of the finished product per square meter was observed and the data was recorded.

[0162] 2. Stability test

[0163] Finished laminated polycarbonate panels were prepared by the preparation methods of Examples 1-6, respectively, with reference to GB257633-2009 Safety Glass for Building Part 3 Laminated Glass, and the initial curvature of each sample was tested to be r1000; the finished products were then placed under natural conditions for 3 years, and the curvature data were recorded again.

[0164] 3. Stability test

[0165] Finished laminated polycarbonate plates were prepared by the preparation methods of Examples 1 to 16, and the tear strength of the TPU film from the surface of the polycarbonate plate was tested with reference to ASTM D-624, and the data were recorded; high tear strength means high bonding stability.

[0166] 4. Quality inspection

[0167] Finished laminated polycarbonate panels were prepared using the preparation methods of Examples 1-14, respectively, and the height of the highest position of the protrusion at the edge of the finished product was measured, and the data of Examples 1-3 and 5 were recorded; and the number of scratches on the surface of the polycarbonate panel on the finished products of Examples 1-3, 12 and Example 18 was recorded, and the data was recorded.

[0168] For each of the above test items, except for the change of the sample, the other test conditions remain unchanged, following the single variable principle.

[0169] Table 1 Performance test table

[0170]

[0171] It can be seen from Examples 1-3 and Table 1 that the finished laminated polycarbonate sheet has a small thickness difference, is basically free of bubbles, is not easy to change in curvature over a long period of time, has a high tear strength, has a small amount of glue on the edge, and has no scratches; this shows that the laminated polycarbonate sheet not only has good quality, but also has high structural stability and a long service life.

[0172] It can be seen from Example 1 and Examples 4-18 and Table 1 that during the preparation process of the laminated polycarbonate sheet in Example 4, the temperature rise in the second stage is 75°C. Compared with Example 1, the laminated polycarbonate sheet in Example 4 has a greater curvature change than that in Example 1 after long-term use or storage, and the tear strength is lower than that in Example 1; this indicates that the TPU film and EVA cannot be hot-melted at 75°C, and the TPU film that plays a bonding role is gradually hot-melted in the third stage, which affects the contact area between the TPU film and the polycarbonate sheet, making it difficult to bond evenly and stably, and easily causing the finished product to straighten.

[0173] During the preparation of the laminated polycarbonate board in Example 5, the temperature was directly raised to 90°C. Compared with Example 1, the thickness difference of the laminated polycarbonate board in Example 5 was greater than that in Example 1, the number of bubbles was greater than that in Example 1, the tear strength was less than that in Example 1, the bulge height was greater than that in Example 1, and the curvature change was greater than that in Example 1; this indicates that directly hot-melting the TPU film and EVA can easily make the TPU film bonded to the polycarbonate board that has not been bent to the specified curvature. When the polycarbonate board is bent to the specified curvature over time, the TPU film is prone to flow and migration due to the existence of the curved surface during this period, affecting the uniformity and bonding stability of the laminated polycarbonate board, and the uneven and unstable bonding can easily make the laminated polycarbonate board straighten out. At the same time, the flowing PU glue can easily produce bulges at the edges of the laminated polycarbonate board, affecting the quality of the finished product.

[0174] In Example 6, there is no polyvinyl alcohol liquid and water-white rosin resin particles on the surface of the polycarbonate board; the coated PMMA particles and polyacrylamide-modified transparent mica sheets are replaced with thermoplastic polyurethane elastomer of equal mass in the TPU film raw material. Compared with Example 1, the thickness difference of the laminated polycarbonate board prepared in Example 6 is greater than that in Example 1, and the tear strength is less than that in Example 1; this indicates that the combination of polyvinyl alcohol liquid, water-white rosin resin, coated PMMA particles and polyacrylamide-modified transparent mica sheets can improve the bonding stability and bonding strength of the laminated polycarbonate board, and utilize the adsorption effect of each other to avoid the TPU film from flowing between the polycarbonate boards as much as possible, which affects the uniformity and quality of the finished product.

[0175] No water-white rosin resin particles were added to the raw materials of the polycarbonate board in Example 7. Compared with Example 1, the thickness difference of the laminated polycarbonate prepared in Example 7 was greater than that in Example 1, and the tear strength was less than that in Example 1. This indicates that the water-white rosin resin particles are not easy to melt and flow during the preparation of the laminated polycarbonate board, and only soften. In addition, the carboxyl group in the water-white rosin resin has a bonding compatibility with the TPU film, which further restrains the TPU film after hot melting and avoids the flow of the TPU film after hot melting, so that the finished laminated polycarbonate board has better quality and stability.

[0176] In Example 8, the water-white rosin resin particles are replaced with EVA particles of equal mass in the raw materials of the polycarbonate board. Compared with Example 1, the thickness difference of the laminated polycarbonate board prepared in Example 8 is greater than that in Example 1, but the tear strength is slightly greater than that in Example 1; this indicates that the viscosity of EVA increases after hot melting, which can improve the bonding strength. Although EVA has a certain viscosity, it also has a certain fluidity after hot melting, so it is easy to make the lamination between the two polycarbonate boards uneven, affecting the quality of the finished product.

[0177] In Example 9, the polyvinyl alcohol liquid is replaced by an equal mass of ethyl cellulose ethanol solution in the raw material of the polycarbonate board. Compared with Example 1, the thickness difference of the laminated polycarbonate board prepared in Example 9 is greater than that in Example 1, and the tear strength is less than that in Example 1; this indicates that the hydroxyl groups in polyvinyl alcohol can attract the amino groups and amide groups in the TPU film, thereby further improving the bonding strength between the TPU film and the polycarbonate board, so that the finished laminated polycarbonate board has better bonding stability and bonding uniformity.

[0178] In Example 10, the coated PMMA particles and the polyacrylamide-modified transparent mica sheets are replaced with the same mass of silicon dioxide in the TPU film raw material. Compared with Example 1, the thickness difference of the laminated polycarbonate board prepared in Example 10 is greater than that in Example 1, and the tear strength is less than that in Example 1; this indicates that silicon dioxide cannot produce stable adhesion with the surface of the polycarbonate board, while the coated PMMA particles and the polyacrylamide-modified transparent mica sheets can produce relatively stable adhesion with the water-white rosin resin particles and polyvinyl alcohol on the surface of the polycarbonate board, thereby improving the bonding stability and bonding strength between the two polycarbonate boards, and preventing the TPU film from flowing after hot melting, so that the finished product has better quality.

[0179] In the preparation process of the coated PMMA particles in the TPU film of Example 11, the sodium carboxymethyl cellulose solution was replaced by an ethyl cellulose ethanol solution of equal mass. Compared with Example 1, the thickness difference of the laminated polycarbonate board prepared in Example 11 was greater than that in Example 1, and the tear strength was less than that in Example 1; this indicates that the carboxyl group in the sodium carboxymethyl cellulose on the surface of the coated PMMA particles can improve the bonding strength between the coated PMMA particles and the thermoplastic polyurethane elastomer and the polyacrylamide-modified transparent mica sheet, and can improve the bonding stability between the coated PMMA particles and the polycarbonate board, thereby improving the quality and service life of the finished laminated polycarbonate board.

[0180] In the preparation process of the coated PMMA particles in the TPU film of Example 12, no EVA particles were added. Compared with Example 1, the thickness difference of the laminated polycarbonate board prepared in Example 12 was greater than that in Example 1, and the tear strength was less than that in Example 1. This shows that the addition of EVA particles can improve the bonding compatibility between PMMA particles and thermoplastic polyurethane elastomer, thereby further improving the bonding stability and bonding strength of the TPU film, so that the laminated polycarbonate board has better processing quality and longer service life.

[0181] During the preparation of the coated PMMA particles in the TPU film of Example 13, the PMMA particles were not etched and not immersed and dispersed by sodium carboxymethyl cellulose solution. Compared with Example 1, the thickness difference of the laminated polycarbonate board prepared in Example 13 was greater than that in Example 1, and the tear strength was less than that in Example 1. This indicates that the etching treatment combined with the adhesion of sodium carboxymethyl cellulose solution can further improve the bonding effect between the PMMA particles and the thermoplastic polyurethane elastomer, thereby improving the bonding stability and bonding strength of the TPU film.

[0182] In Example 14, the modified transparent mica sheets in the TPU film replace the polyacrylamide modified transparent mica sheets. During the preparation of the modified transparent mica sheets, the transparent mica sheets are not treated with polyacrylamide. In Example 15, the modified transparent mica sheets in the TPU film replace the polyacrylamide modified transparent mica sheets. During the preparation, the transparent mica sheets are treated with ethyl cellulose ethanol solution. Compared with Example 1, the thickness difference of the laminated polycarbonate plates prepared in Examples 14 and 15 is greater than that in Example 1, and the tear strength is less than that in Example 1. This indicates that the combination of polyacrylamide, sodium carboxymethyl cellulose and transparent mica sheets can improve the bonding stability between the transparent mica sheets and the thermoplastic polyurethane elastomer, and the polyacrylamide modified transparent mica sheets can have a stable bonding with the polycarbonate sheet, thereby further preventing the hot-melt TPU film from hot-melting to ensure the quality of the finished product.

[0183] During the preparation of the PET high-temperature tape in Example 16, polyamide resin particles were not added to the adhesive raw material. Compared with Example 1, the thickness difference of the laminated polycarbonate board prepared in Example 16 was greater than that in Example 1, and the tear strength was less than that in Example 1; this indicates that the elastic buffering effect of the polyamide resin particles can prevent the TPU film from flowing out of the surface of the polycarbonate board and generating bulges, thereby easily affecting the fixing effect and affecting the quality and stability of the finished product.

[0184] In Example 17, no alumina powder is added to the TPU isolation film. Compared with Example 1, the thickness difference of the laminated polycarbonate board prepared in Example 17 is greater than that in Example 1, which indicates that alumina powder has a heat transfer effect and can ensure that heat is evenly distributed on the polycarbonate board and the TPU film, thereby ensuring the uniform bonding of the finished product.

[0185] In Example 18S3, no TPU isolation film was added. Compared with Example 1, the laminated polycarbonate board prepared in Example 18 was more seriously scratched, indicating that the addition of TPU isolation film can protect the surface of the polycarbonate board from being scratched by the curved glass mold.

[0186] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A high pressure forming method for laminated polycarbonate sheets, characterized in that: The steps include: S1, heating two glasses to 600-700° C. to prepare a curved glass mold; S2, laying a TPU film between two polycarbonate plates to obtain a laminated part; S3, placing the laminated part between two curved glass molds, and then fixing it to obtain a fixed part; S4, the fixing parts are subjected to vacuum cold extraction treatment, and then subjected to high temperature and high pressure treatment at a temperature of 50-135°C and a pressure of 0.05-1.2MPa for 160-260min, and then the curved glass mold is removed to obtain a laminated polycarbonate board; The TPU film is prepared by the following method: Weigh 60-90 parts of thermoplastic polyurethane elastomer, 1-5 parts of coated PMMA particles, and 1-5 parts of polyacrylamide-modified transparent mica sheets, mix and stir evenly, and perform molding treatment to obtain a TPU film; The coated PMMA particles are prepared by the following method: Weigh PMMA particles, etch them, and then place them in a 0.1-0.5% sodium carboxymethyl cellulose solution for dispersion and immersion, take them out and dry them to obtain loaded PMMA particles; The EVA particles are immersed and dispersed in a 0.5-1% sodium carboxymethyl cellulose aqueous solution, and then the EVA particles are taken out to obtain loaded EVA particles; The loaded EVA particles are uniformly sprayed on the surface of the loaded PMMA particles at a mass ratio of 1:1-2, and the finished product is obtained after drying.

2. A high pressure forming method for laminated polycarbonate sheets according to claim 1, characterized in that: The vacuum pressure of the vacuum cold pumping treatment in S4 is -0.08 to -0.1 MPa, and the time is 4 to 8 hours.

3. The high pressure forming method of a laminated polycarbonate sheet according to claim 1, characterized in that: The specific steps of the high temperature and high pressure treatment in S4 are as follows: Raise the temperature to 50-60℃ while introducing air at a pressure of 0.05-0.15MPa, maintain for 50-90min, then raise the temperature to 90-100℃, maintain for 50-90min at a pressure of 0.1-0.2MPa, finally raise the temperature to 125-135℃, maintain for 60-80min at a pressure of 1.1-1.2MPa; then keep the pressure unchanged, cool to below 50℃, and exhaust to normal pressure.

4. The high pressure forming method of laminated polycarbonate sheet according to claim 1, characterized in that: The polycarbonate plate is prepared by the following method: Polyvinyl alcohol liquid is evenly sprayed on the surface of a commercially available polycarbonate plate at a mass ratio of 1:0.02-0.06, and then water-white rosin resin particles are evenly sprayed. The mass ratio of the commercially available polycarbonate plate to the water-white rosin resin particles is 1:0.1-0.

22. After drying, a finished product is obtained.

5. The high pressure forming method of laminated polycarbonate sheet according to claim 1, characterized in that: In the S3, PET high temperature tape is used for fixing.

6. A high pressure forming method for laminated polycarbonate sheets according to claim 5, characterized in that: The PET high temperature tape is prepared by the following method: The adhesive is sprayed evenly on the PET substrate and rolled to obtain a finished product; the adhesive is composed of organic silicone adhesive and polyamide resin particles in a mass ratio of 1:0.05-0.

2.

7. The high pressure forming method of laminated polycarbonate sheet according to claim 1, characterized in that: A TPU isolation film is provided between the laminated component and the two curved glass molds in S3.

8. The high pressure forming method of laminated polycarbonate sheet according to claim 7, characterized in that: The TPU isolation film is prepared by the following method: Thermoplastic polyurethane elastomer and aluminum oxide powder are weighed and mixed in a mass ratio of 1:0.02-0.06, and stirred evenly, and molded to obtain a finished product.

Citation Information

Patent Citations

  • Fully transparent composite riot shield and preparation method therefor

    CN103471465A

  • Ordered vertical channel double-pass film preparation method and product thereof

    CN105271109A

  • Processing method for curved-surface dual-glass assembly

    CN105489701A

  • Preparation method of integrally molded curved touch screen

    CN106648243A

  • Solar cell module

    CN108336229A