A concrete quick repair material and its preparation method and application

By using specific proportions of raw materials such as ultrafine cement and lightly simmered magnesium oxide, the initial reaction rate and bonding strength are improved, the problem of slow hydration of ordinary silicate cement-based repair materials is solved, and the rapid repair of concrete is achieved The rapid condensation and high strength of the material simplifies the construction process.

CN116199485BActive Publication Date: 2024-11-26SICHUAN HUASHI GREEN HOMELAND BUILDING MATERIALS
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211094289.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-08
Publication Date
2024-11-26
Estimated Expiration
2042-09-08

AI Technical Summary

Technical Problem

In the prior art, the initial reaction rate of ordinary silicate cement-based repair materials is slow, the repair cycle is long, and the bonding strength is low, resulting in the concrete repair being unsolid and the problem of re-damage is prone to occur.

Method used

Using ultrafine cement, lightly flammed magnesium oxide, fly ash, silicon powder, quartz sand and triethanolamine, a reaction rate and bonding strength in the early stage of hydration are increased through specific weight ratios and preparation methods, and a reaction rate and bonding strength are designed. Quick refinishing materials for concrete that can quickly condense.

Benefits of technology

The reaction rate and bond strength are improved in the early stage of hydration. The materials can quickly condense during construction, simplify the repair process, and significantly improve the compressive strength and fluidity, solving the difficulties of traditional materials in construction. and quality issues.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention discloses a concrete quick repair material and a preparation method and application thereof, which belongs to the technical field of building materials, and solves the problems of slow initial hydration reaction rate, long repair cycle and low bonding strength of ordinary silicate cement-based repair materials in the prior art. The raw materials of the concrete quick repair material of the invention include ultrafine cement, light-burned magnesium oxide, fly ash, silica powder, quartz sand, water reducer and triethanolamine in a certain weight ratio. The preparation method of the invention is: after premixing ultrafine cement, light-burned magnesium oxide, fly ash, silica powder and quartz sand, add water reducer and water and stir evenly; add triethanolamine and stir before use to obtain the material. The concrete quick repair material of the invention does not coagulate before use, and can quickly coagulate by adding a small amount of admixture after arriving at the construction site, exert strength, and meet the use requirements at the fastest speed. The concrete quick repair material of the invention has good fluidity and can reach a self-compacting state without vibration.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of building materials, and in particular relates to a concrete rapid repair material and a preparation method and application thereof. Background Art

[0002] Because cement concrete is affected by various environmental factors, it will also be damaged to varying degrees during its service life, causing various problems, and some may even pose safety hazards. Cement concrete repair materials can be divided into inorganic and organic materials according to their chemical composition. Organic repair materials use high molecular polymers as the main raw materials, and have the advantages of chemical corrosion resistance, impact resistance, and high bonding strength. However, they are expensive, have high heat generation in the early stage, and the hardened slurry is brittle and shrinks relatively large. In addition, the compatibility of polymers with the substrate is poor and they are prone to falling off. In addition, organic materials are prone to aging under environmental influences and have poor durability.

[0003] Although traditional inorganic mineral polymer-based rapid repair mortar has high early strength and fast strength development in the later stage, it is also accompanied by the problem of premature setting time. The premature setting time causes construction difficulties for long-distance repairs and road repairs with many cracks, which greatly limits the use and promotion of inorganic mineral polymer-based rapid repair mortar. Ordinary Portland cement-based inorganic repair materials have the advantages of low cost, environmental protection, and low price. They are consistent with the performance of old concrete and have been widely used in actual production. However, the initial hydration reaction rate of ordinary Portland cement is slow, the repair cycle is long, and the bonding strength is low, which can easily cause the new and old interfaces to be weakly bonded and cracked, thereby causing quality problems such as re-damage of concrete.

[0004] Therefore, providing a cement-based repair material for cement concrete that can enhance the initial hydration reaction rate and improve the bonding strength has become an urgent problem to be solved by those skilled in the art. Summary of the invention

[0005] One of the purposes of the present invention is to provide a rapid concrete repair material to solve the problems of slow initial hydration reaction rate, long repair period and low bonding strength of ordinary Portland cement-based repair materials in the prior art.

[0006] The second object of the present invention is to provide a method for preparing the concrete rapid repair material.

[0007] The third object of the present invention is to provide an application of the concrete rapid repair material.

[0008] To achieve the above object, the technical solution adopted by the present invention is:

[0009] The invention provides a concrete rapid repair material, the raw materials of which include: ultrafine cement, light-burned magnesium oxide, fly ash, silica fume, quartz sand, water reducing agent and triethanolamine; the weight ratio of each raw material is:

[0010]

[0011] The amount of water reducing agent is 0.5-1.0wt.% of the total weight of ultrafine cement, fly ash and silica fume;

[0012] The dosage of triethanolamine is 0.3-0.7wt.% based on the total weight of ultrafine cement, fly ash and silica fume.

[0013] In some embodiments of the present invention, the raw materials include: ultrafine cement, light-burned magnesium oxide, fly ash, silica fume, quartz sand, water reducer and triethanolamine; the weight ratio of each raw material is:

[0014]

[0015] The amount of water reducing agent is 0.6-0.8wt.% of the total weight of ultrafine cement, fly ash and silica fume;

[0016] The dosage of triethanolamine is 0.5wt.% of the total weight of ultrafine cement, fly ash and silica fume.

[0017] In some embodiments of the present invention, the raw materials include: ultrafine cement, light-burned magnesium oxide, fly ash, silica fume, quartz sand, water reducer and triethanolamine; the weight ratio of each raw material is:

[0018]

[0019] The amount of water reducing agent is 0.6-0.8wt.% of the total weight of ultrafine cement, fly ash and silica fume;

[0020] The dosage of triethanolamine is 0.5wt.% of the total weight of ultrafine cement, fly ash and silica fume.

[0021] In some embodiments of the present invention, the specific surface area of ​​the ultrafine cement is 800 to 1000 m 2 / kg; preferably 900m 2 / kg.

[0022] In some embodiments of the present invention, the ultrafine cement is made by grinding No. 42.5 cement or No. 52.5 cement.

[0023] In some embodiments of the present invention, the reaction activity of the light-burned magnesium oxide is 100-150S.

[0024] The silicon powder described in the present invention is non-condensed silicon powder, and the silicon dioxide content is ≥92wt.%.

[0025] In some embodiments of the present invention, the quartz sand has two gradations of fineness of 40-70 mesh and 20-40 mesh, and the mass ratio thereof is 1-3:7-9, preferably 2:8.

[0026] The water reducing agent described in the present invention is a polycarboxylic acid water reducing agent.

[0027] The present invention provides a method for preparing a concrete rapid repair material, comprising the following steps:

[0028] Step 1. Prepare the raw materials in proportion;

[0029] Step 2. Put ultrafine cement, light-burned magnesium oxide, fly ash, silica fume and quartz sand into a premixer for premixing to obtain a premix;

[0030] Step 3. Add water reducing agent and water to the premix and stir evenly;

[0031] Step 4. Add triethanolamine and stir to obtain the product.

[0032] In some embodiments of the present invention, in step 3, the amount of water added is 18-25 wt.% of the total weight of ultrafine cement, fly ash and silica fume, preferably 20 wt.%.

[0033] In some embodiments of the present invention, in step 4, triethanolamine is added before the repair perfusion;

[0034] Preferably, after adding triethanolamine, rapid stirring is performed for 15 to 60 seconds, more preferably for 30 seconds.

[0035] The application of the concrete rapid repair material provided by the present invention in rapid building repair is preferably applied to concrete pavement repair, basement structure leakage repair, concrete cement pavement repair, and bridge repair.

[0036] Compared with the prior art, the present invention has the following beneficial effects:

[0037] The invention is scientifically designed and ingeniously conceived. The concrete quick repair material of the invention does not solidify before use, but can quickly solidify by adding a small amount of admixture after arriving at the construction site, exerting strength and meeting the use requirements at the fastest speed.

[0038] The applicant has also unexpectedly discovered that the concrete rapid repair material of the present invention has excellent fluidity and can achieve a self-compacting state without vibration, which greatly simplifies the repair process. DETAILED DESCRIPTION

[0039] In order to make the purpose, technical scheme and advantages of the present invention more clear, the present invention is further described in detail below. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0040] Unless otherwise specified, the parts described in the embodiments of the present invention refer to parts by mass.

[0041] Example 1

[0042] This embodiment discloses a method for preparing the concrete rapid repair material of the present invention. The raw materials of the concrete rapid repair material of this embodiment are:

[0043]

[0044] The ultrafine cement of this embodiment is made by grinding No. 42.5 cement; the silica powder is non-agglomerated silica powder, and the silicon dioxide content is ≥92wt.%; the fineness of quartz sand is 40-70 mesh and 20-40 mesh, and the mass ratio is 2:8.

[0045] The preparation method is as follows: after ultrafine cement, lightly burned magnesium oxide, fly ash, silica powder and quartz sand are mixed evenly, polycarboxylate water reducer and 30 parts of water are added and stirred evenly. When reaching the use site, triethanolamine is added and stirred quickly for 30 seconds with a hand-held mixer to obtain a concrete quick repair material.

[0046] Example 2

[0047] This embodiment discloses a method for preparing a quick concrete repair material of the present invention. Compared with Embodiment 1, the specific surface area of ​​the ultrafine cement in this embodiment is different, and the other conditions are the same. The specific surface area of ​​the ultrafine cement in this embodiment is 100 Kg / m 2 .

[0048] Comparative Example 1

[0049] Compared with Example 1, this comparative example uses No. 42.5 cement instead of superfine cement, and the other conditions are the same.

[0050] Test Example 1

[0051] Ordinary Portland cement (No. 42.5 cement), the concrete quick repair materials prepared in Examples 1 and 2, and the concrete quick repair materials prepared in Comparative Example 1 were tested for performance, wherein the setting time and strength tests were performed in accordance with JGJ / T70-2009 "Basic Performance Test Methods for Building Mortar", and the flow properties were tested in accordance with JG / T 985-2017 "Cement-based Self-leveling Mortar for Ground Use". The results are shown in the following table:

[0052] Table 1

[0053] Ordinary Portland Cement Comparative Example 1 Example 1 Example 2 Fluidity / mm 100 150 155 150 Initial setting time / min 120 65 10 8 Final setting time / min 320 210 18 15 1h compressive strength / MPa 0 0 5 12 2h compressive strength / MPa 0 0 15 20 3h compressive strength / MPa 0 0 24.5 38 4h compressive strength / MPa 0 3 35 42 8h compressive strength / MPa 7.2 15 48 55 1d compressive strength / MPa 15.3 24 80 84

[0054] As shown in Table 1, the concrete quick repair material of the present invention can set in a short time and has early strength compared with ordinary silicate cement and the modified material of comparative example 1. The initial setting time and final setting time of Example 2 are both shorter than those of Example 1, and the compressive strength at the same time point is higher than that of Example 1, indicating that the larger the surface area of ​​the cement, the more fully the cement is hydrated, and the better its early strength performance.

[0055] In addition, the concrete rapid repair material made of high-surface-area ultrafine cement of the present invention has the same fluidity as the repair material made of ordinary Portland cement in Comparative Example 1, breaking the technical prejudice in the prior art that the larger the cement surface area, the worse the fluidity of the mortar produced. The present invention has unexpected technical effects.

[0056] Example 3

[0057] This embodiment discloses a method for preparing the concrete rapid repair material of the present invention. The raw materials of the concrete rapid repair material of this embodiment are:

[0058] The raw materials of the concrete quick repair material of this embodiment are:

[0059]

[0060]

[0061] The ultrafine cement of this embodiment is made by grinding No. 52.5 cement; the silica powder is non-agglomerated silica powder, and the silicon dioxide content is ≥92wt.%; the fineness of quartz sand is 40-70 mesh and 20-40 mesh, and the mass ratio is 2:8.

[0062] The preparation method is as follows: after ultrafine cement, lightly burned magnesium oxide, fly ash, silica powder and quartz sand are mixed evenly, polycarboxylate water reducer and 33 parts of water are added and stirred evenly. When reaching the use site, triethanolamine is added and stirred quickly for 50 seconds with a handheld mixer to obtain a concrete quick repair material.

[0063] Example 4

[0064] This embodiment discloses a method for preparing the concrete rapid repair material of the present invention. The raw materials of the concrete rapid repair material of this embodiment are:

[0065]

[0066] The ultrafine cement of this embodiment is made by grinding No. 52.5 cement; the silica powder is non-agglomerated silica powder, and the silicon dioxide content is ≥92wt.%; the fineness of quartz sand is 40-70 mesh and 20-40 mesh, and the mass ratio is 2:8.

[0067] The preparation method is as follows: after ultrafine cement, lightly burned magnesium oxide, fly ash, silica powder and quartz sand are mixed evenly, polycarboxylate water reducer and 31 parts of water are added and stirred evenly. When reaching the use site, triethanolamine is added and stirred quickly for 20 seconds with a handheld mixer to obtain a concrete quick repair material.

[0068] Example 5

[0069] This embodiment discloses a method for preparing the concrete rapid repair material of the present invention. The raw materials of the concrete rapid repair material of this embodiment are:

[0070]

[0071]

[0072] The ultrafine cement of this embodiment is made by grinding No. 52.5 cement; the silica powder is non-agglomerated silica powder, and the silicon dioxide content is ≥92wt.%; the fineness of quartz sand is 40-70 mesh and 20-40 mesh, and the mass ratio is 2:8.

[0073] The preparation method is as follows: after ultrafine cement, lightly burned magnesium oxide, fly ash, silica powder and quartz sand are mixed evenly, polycarboxylate water reducer and 36 parts of water are added and stirred evenly. When reaching the use site, triethanolamine is added and stirred rapidly for 60 seconds with a hand-held mixer to obtain a concrete quick repair material.

[0074] Example 6

[0075] This embodiment discloses a method for preparing the concrete rapid repair material of the present invention. The raw materials of the concrete rapid repair material of this embodiment are:

[0076]

[0077] The ultrafine cement of this embodiment is made by grinding No. 42.5 cement; the silica powder is non-agglomerated silica powder, and the silicon dioxide content is ≥92wt.%; the fineness of quartz sand is 40-70 mesh and 20-40 mesh, and the mass ratio is 2:8.

[0078] The preparation method is as follows: after ultrafine cement, lightly burned magnesium oxide, fly ash, silica powder and quartz sand are mixed evenly, polycarboxylate water reducer and 35 parts of water are added and stirred evenly. When reaching the use site, triethanolamine is added and stirred quickly for 30 seconds with a hand-held mixer to obtain a concrete quick repair material.

[0079] Test Example 2

[0080] The concrete quick repair materials prepared in Examples 3 to 6 were subjected to performance tests, wherein the setting time and strength tests were conducted in accordance with JGJ / T 70-2009 "Basic performance test methods for building mortar", and the flow properties were tested in accordance with JG / T 985-2017 "Cement-based self-leveling mortar for floor use". The results are shown in the following table:

[0081] Table 2

[0082] Example 3 Example 4 Example 5 Example 6 Fluidity / mm 145 150 160 155 Initial setting time / min 9 20 6 7 Final setting time / min 16 31 12 18 1h compressive strength / MPa 7 3 20 6 2h compressive strength / MPa 17 10 33 14 3h compressive strength / MPa 34.2 18 45 25 4h compressive strength / MPa 38.4 27.5 52 38 8h compressive strength / MPa 50 42.7 73 50 1d compressive strength / MPa 80.1 60.9 102 75

[0083] Finally, it should be noted that the above embodiments are only preferred embodiments of the present invention to illustrate the technical solution of the present invention, but not to limit it, and certainly not to limit the patent scope of the present invention. Any changes or modifications that have no substantial significance on the main design concept and spirit of the present invention, which solve technical problems consistent with the present invention, should be included in the protection scope of the present invention; in addition, the direct or indirect application of the technical solution of the present invention in other related technical fields should also be included in the patent protection scope of the present invention.

Claims

1. A concrete rapid repair material, characterized in that: The raw materials are: ultrafine cement, light-burned magnesium oxide, fly ash, silica fume, quartz sand, water reducing agent and triethanolamine; the weight ratio of each raw material is: 90~130 parts of ultrafine cement, 15~35 parts of fly ash, 15~35 parts of silicon powder, 90~130 parts of quartz sand, Lightly calcined magnesium oxide 10-20 parts, The dosage of water reducing agent is 0.5~1.0 wt.% of the total weight of ultrafine cement, fly ash and silica fume; The dosage of triethanolamine is 0.3-0.8wt.% of the total weight of ultrafine cement, fly ash and silica fume; The specific surface area of ​​the ultrafine cement is 800-1000m 2 / kg; The quartz sand has two gradations of fineness: 40-70 mesh and 20-40 mesh, and the mass ratio thereof is 1-3:7-9.

2. A concrete rapid repair material according to claim 1, characterized in that: The raw materials are: ultrafine cement, light-burned magnesium oxide, fly ash, silica fume, quartz sand, water reducing agent and triethanolamine; the weight ratio of each raw material is: 100~120 parts of ultrafine cement, 20~30 parts of fly ash, 20~30 parts of silicon powder, 100~130 parts of quartz sand, Lightly calcined magnesium oxide 10-20 parts, The dosage of water reducing agent is 0.6~0.8 wt.% of the total weight of ultrafine cement, fly ash and silica fume; The dosage of triethanolamine is 0.5wt.% of the total weight of ultrafine cement, fly ash and silica fume.

3. A concrete rapid repair material according to claim 1, characterized in that: The raw materials are: ultrafine cement, light-burned magnesium oxide, fly ash, silica fume, quartz sand, water reducing agent and triethanolamine; the weight ratio of each raw material is: 100 parts of ultrafine cement, 20 parts of fly ash, 30 parts of silicon powder, 100 parts of quartz sand, 15 parts of light-burned magnesium oxide, The dosage of water reducing agent is 0.6~0.8 wt.% of the total weight of ultrafine cement, fly ash and silica fume; The dosage of triethanolamine is 0.5wt.% of the total weight of ultrafine cement, fly ash and silica fume.

4. A concrete rapid repair material according to any one of claims 1 to 3, characterized in that: The specific surface area of ​​the ultrafine cement is 900 m 2 / kg.

5. A concrete rapid repair material according to claim 4, characterized in that: The ultrafine cement is made by grinding No. 42.5 cement or No. 52.5 cement.

6. A concrete rapid repair material according to any one of claims 1 to 3, characterized in that: The reaction activity of the light-burned magnesium oxide is 100-150S.

7. A method for preparing a concrete rapid repair material according to any one of claims 1 to 6, characterized in that: The following steps are involved: Step 1. Prepare the raw materials according to the proportion; Step 2. Put ultrafine cement, light-burned magnesium oxide, fly ash, silica fume and quartz sand into a premixer for premixing to obtain a premix; Step 3. Add water reducing agent and water to the premix and stir evenly; Step 4. Add triethanolamine and stir to obtain the product.

8. The preparation method according to claim 7, characterized in that: In step 3, the water content is 18-25wt.% of the total weight of ultrafine cement, fly ash and silica fume.

9. The preparation method according to claim 7, characterized in that: In step 3, the water content is 20 wt.% of the total weight of ultrafine cement, fly ash and silica fume.

10. The preparation method according to claim 7, characterized in that: In the step 4, triethanolamine is added before the repair perfusion.

11. The preparation method according to claim 10, characterized in that: After adding triethanolamine, stir rapidly for 15 to 60 seconds.

12. The preparation method according to claim 10, characterized in that: After adding triethanolamine, stir rapidly for 30 seconds.

13. Use of the concrete rapid repair material according to any one of claims 1 to 5 in rapid repair of buildings.

14. The use according to claim 13, characterized in that Application in concrete pavement repair, basement structure leakage repair, concrete cement pavement repair and bridge repair.