A method for preparing ceramic powder
Through the vaporization and reaction of the radio frequency plasma device in the plasma generating chamber, the complexity and purity problems of ceramic powder preparation are solved, the preparation of ceramic powder with high purity and fine particle size is achieved, the process is simplified and the uniformity and purity of the product are improved. Transparency.
Patent Information
- Application Number
- CN202111458695.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-12-01
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2041-12-01
AI Technical Summary
The existing ceramic powder preparation method is complex and the process is long, making it difficult to prepare fine-grained and high-purity magnesia-aluminum spinel ceramic powder, and there are by-products and pore impurities that affect the transparency.
A radio frequency plasma device is used to vaporize solid raw materials in the plasma generating chamber, and the gaseous raw materials react with the dissociated reactive gases. Ceramic powder is obtained through condensation, and high-temperature plasma and stable thermal plasma are used to control the reaction to ensure product quality. uniformity and purity, and control the stoichiometric ratio by adjusting the oxygen ratio.
It achieves the preparation of ceramic powder with high purity (≥99.999%) and fine particle size (20 nanometers to 300 nanometers), simplifies the process, avoids by-products, and improves the uniformity and transparency of the chemical composition of the ceramic powder.
Smart Images

Figure CN116199507B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of materials and manufacturing, and in particular to a method for preparing ceramic powder. Background Art
[0002] Common ceramic materials in daily life are usually opaque, because ceramics are an inorganic polycrystalline material. Due to the large number of defects such as pores and impurities inside the ceramics, the light incident on the ceramics is scattered and refracted, so that the incident light cannot pass through the ceramics. Transparent magnesium aluminum spinel ceramics are a new type of ceramics that have been studied a lot in recent years. As an advanced ceramic material with both good light transmittance and excellent mechanical properties, it has become a basic material and key material in aerospace, traffic lighting, electronic instruments, various observation and detection windows and other technical fields due to its unique excellent properties.
[0003] The preparation of transparent magnesium-aluminum spinel ceramics requires very high purity of ceramic powder, and the particle size needs to reach the level of nanopowder to achieve a sufficiently high sintering density. At the same time, the light transmittance of transparent magnesium-aluminum spinel ceramics requires no bubbles on the grain boundaries, because pores and impurities will scatter light and affect its transparency.
[0004] There are many methods for preparing magnesium aluminum spinel powder, mainly high temperature solid phase method, solution-solid phase method, sol-gel method, supercritical fluid method, co-precipitation method and spark plasma sintering method, etc. At present, most of the processes for preparing magnesium aluminum spinel ceramic powder are complicated, long, and have by-products, making it difficult to prepare fine particle size and high purity powder.
[0005] In conclusion, the existing ceramic powder preparation methods need to be further improved. Summary of the invention
[0006] The technical problem solved by the invention is to provide a method for preparing ceramic powder to improve the performance of the ceramic powder.
[0007] In order to solve the above technical problems, the technical solution of the present invention provides a method for preparing ceramic powder, comprising: providing a plasma device, the plasma device comprising: a radio frequency plasma power supply, a reaction chamber and a plasma generating chamber located at the top of the reaction chamber, and the plasma generating chamber is connected to the reaction chamber; performing a first ventilation, introducing a first gas into the plasma generating chamber, and using a radio frequency plasma power supply to dissociate the first gas; after the first ventilation, performing a second ventilation, continuing to introduce the first gas into the plasma generating chamber, and introducing a reaction gas into the plasma generating chamber at the same time, and using a radio frequency plasma power supply to dissociate the first gas and the reaction gas to form a mixed gas plasma; providing a solid raw material, the solid raw material comprising two or more elemental metals; after forming the mixed gas plasma, sending the solid raw material to the plasma generating chamber, the solid raw material is vaporized in the plasma generating chamber to form a gaseous raw material, the gaseous raw material reacts with the dissociated reaction gas in the reaction chamber to generate a process product; and obtaining the ceramic powder by condensing the process product.
[0008] Optionally, the plasma generating chamber has a main air inlet and a side air inlet, and the side air inlet is located at the edge of the plasma generating chamber relative to the main air inlet; the ceramic powder preparation method also includes: in the first ventilation stage, the first gas is introduced from the main air inlet and the side air inlet; in the second ventilation stage, the flow rate of the first gas in the main air inlet remains unchanged, the first gas is introduced from the side air inlet at a set reduced speed, and the reaction gas is introduced from the side air inlet at the same time.
[0009] Optionally, the process parameters of the first ventilation stage include: a power output range of 30 kW to 60 kW, a gas pressure range of 50 kPa to 80 kPa in the reaction chamber, a flow rate range of 3 m / s to 40 m / s, and a flow rate of 10 m / s to 80 m / s. 3 / h to 10m 3 / h; the process parameters of the second ventilation stage include: the power output range of the power supply is 40kW to 100kW, the gas pressure range of the reaction chamber is 80kPa to 110kPa, the first gas flow range is 3m 3 / h to 4m 3 / h, the flow range of the reaction gas is 2m 3 / h to 6m 3 / h.
[0010] Optionally, the first gas includes argon, and the reaction gas includes oxygen.
[0011] Optionally, in the mixed gas plasma, the volume ratio of oxygen to the total gas volume ranges from 5% to 85%.
[0012] Optionally, the solid raw material includes metallic aluminum and metallic magnesium.
[0013] Optionally, the molar ratio of aluminum element to magnesium element in the solid raw material ranges from 1:1.81 to 1:2.17.
[0014] Optionally, the solid raw material is in the form of one or more of powder, filament, wire, rod, and tube.
[0015] Optionally, the solid raw material is an aluminum-magnesium alloy.
[0016] Optionally, the material of the ceramic powder is aluminum-magnesium spinel; the ceramic powder is a spherical powder; except for magnesium and aluminum metals, the purity of the ceramic powder is greater than or equal to 99.999%; the particle size distribution of the ceramic powder: D50 ranges from 20 nanometers to 300 nanometers, wherein the ratio of D90 to D50 is less than 3, and the ratio of D10 to D50 is greater than 0.3.
[0017] Optionally, the solid raw material is fed to the plasma generating chamber at a speed of 1 kg / h to 15 kg / h.
[0018] Optionally, the purity of the solid raw material is greater than or equal to 99.999%.
[0019] Optionally, the method of feeding the solid raw material into the plasma generating chamber includes: adding the solid raw material from the outside of the plasma generating chamber to the inside of the plasma generating chamber through a feeding device or pre-setting the solid raw material in the plasma generating chamber.
[0020] Optionally, the purity range of the gas source of the mixed gas plasma is greater than or equal to 99.999%.
[0021] Compared with the prior art, the technical solution of the embodiment of the present invention has the following beneficial effects:
[0022] In the ceramic powder preparation method provided by the technical solution of the present invention, the solid raw material is sent to the plasma generating chamber, the solid raw material is vaporized in the plasma generating chamber to form a gaseous raw material, the gaseous raw material reacts with the dissociated reaction gas in the reaction chamber to generate a process product, and the ceramic powder is obtained by condensing the process product. On the one hand, a radio frequency plasma power supply is used to form a high-temperature plasma, and there is no secondary pollution of the electrode. The radio frequency plasma flame can fully heat the raw material and the atmosphere of the reaction chamber is controllable, which is conducive to improving the uniformity and purity of the product; on the other hand, a stable thermal plasma is generated in the reaction chamber, which is conducive to controlling the uniformity of the product; furthermore, the reaction gas is dissociated as a plasma to provide a reaction heat source, and also as a reaction gas to react with the raw material to form a process product, the process is simple, and there are no by-products; in addition, the solid raw material includes more than two elemental metals, and the molar ratio value between the elemental metals in the solid raw material can be set to be consistent with the molar ratio between the metal elements in the target ceramic powder, and the target ceramic powder with standard stoichiometry can be obtained, which is conducive to improving the uniformity of the chemical composition of the ceramic powder.
[0023] Furthermore, in the mixed gas plasma, the volume ratio of oxygen to the total gas volume ranges from 5% to 85%. Controlling the content of oxygen plasma is beneficial to controlling the reaction process rate and preventing the stoichiometric ratio of the generated ceramic powder components from deviating from the target.
[0024] Furthermore, in the second ventilation stage, the power range of the power supply is controlled within a range of 40 kW to 100 kW, which is beneficial for controlling the energy density of the plasma within a reasonable range and preventing different types of metal atoms from volatilizing or agglomerating in the plasma torch. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 is a flow chart of a method for preparing ceramic powder in one embodiment of the present invention;
[0026] Figure 2 It is a schematic structural diagram of a ceramic powder device in one embodiment of the present invention. DETAILED DESCRIPTION
[0027] As described in the background art, most of the current processes for preparing magnesium aluminum spinel ceramic powders are complex and long, and produce by-products. It is difficult to prepare fine-particle high-purity powders, and the existing ceramic powder preparation methods need to be further improved.
[0028] In order to solve the above problems, the technical solution of the present invention provides a method for preparing ceramic powder, wherein a solid raw material is sent to the plasma generating chamber, the solid raw material is vaporized in the plasma generating chamber to form a gaseous raw material, the gaseous raw material reacts with the dissociated reaction gas in the reaction chamber to generate a process product, and the ceramic powder is obtained by condensing the process product. On the one hand, a high-temperature plasma is formed by using a radio frequency plasma power supply, and there is no secondary pollution of the electrode. The radio frequency plasma flame can fully heat the raw material and the atmosphere of the reaction chamber is controllable, which is conducive to improving the uniformity and purity of the product; on the other hand, a stable thermal plasma is generated in the reaction chamber, which is conducive to controlling the uniformity of the product; furthermore, the reaction gas is dissociated as a plasma to provide a reaction heat source, and also as a reaction gas to react with the raw material to form a process product, the process is simple, and there are no by-products; in addition, the solid raw material includes more than two elemental metals, and the molar ratio value between each elemental metal in the solid raw material can be set to be consistent with the molar ratio between each metal element in the target ceramic powder, and the target ceramic powder with standard stoichiometry can be obtained, which is conducive to improving the uniformity of the chemical composition of the ceramic powder.
[0029] In order to make the above-mentioned objects, features and beneficial effects of the present invention more obvious and easy to understand, specific embodiments of the present invention are described in detail below with reference to the accompanying drawings.
[0030] Figure 1 1 is a flow chart of a method for preparing ceramic powder in one embodiment of the present invention.
[0031] Please refer to Figure 1 , the ceramic powder preparation method comprises the following steps:
[0032] Step S101, providing a plasma device, wherein the plasma device comprises: a radio frequency plasma power supply, a reaction chamber, and a plasma generating chamber located at the top of the reaction chamber, and the plasma generating chamber is connected to the reaction chamber;
[0033] Step S102, performing first ventilation, introducing a first gas into the plasma generating chamber, and using a radio frequency plasma power source to dissociate the first gas;
[0034] Step S103, after the first ventilation, performing the second ventilation, continuing to introduce the first gas into the plasma generating chamber, introducing the reaction gas into the plasma generating chamber at the same time, and using a radio frequency plasma power source to dissociate the first gas and the reaction gas to form a mixed gas plasma;
[0035] Step S104, providing a solid raw material, wherein the solid raw material includes two or more elemental metals;
[0036] Step S105, after the mixed gas plasma is formed, the solid raw material is sent to the plasma generating chamber, the solid raw material is vaporized in the plasma generating chamber to form a gaseous raw material, and the gaseous raw material reacts with the dissociated reaction gas in the reaction chamber to generate a process product;
[0037] Step S106, obtaining ceramic powder by condensing the process product.
[0038] The following is a detailed description with reference to the accompanying drawings.
[0039] Figure 2 It is a schematic structural diagram of a ceramic powder device in one embodiment of the present invention.
[0040] Execute step S101, please refer to Figure 2 , a plasma device is provided, which includes: a radio frequency plasma power supply 200, a reaction chamber (not shown in the figure) and a plasma generating chamber 201 located at the top of the reaction chamber, and the plasma generating chamber 201 is connected to the reaction chamber.
[0041] The plasma generating chamber 201 has a main air inlet 202 and a side air inlet 203 . The side air inlet 203 is located at the edge of the plasma generating chamber 201 relative to the main air inlet 202 .
[0042] The radio frequency plasma power supply 200 is used to electrolyze the gas in the plasma generating chamber 201 to convert it into plasma.
[0043] Please continue to refer to Figure 1 and Figure 2 , perform first ventilation, introduce a first gas into the plasma generating chamber 201, and use a radio frequency plasma power supply 200 to dissociate the first gas.
[0044] In this embodiment, the first gas includes argon.
[0045] Specifically, in the first ventilation stage, the first gas is introduced from the main air inlet 202 and the side air inlet 203 .
[0046] The process parameters of the first ventilation stage include: the power output range of the power supply is 30kW to 60kW, the gas pressure range of the reaction chamber is 50kPa to 80kPa, the flow range of the first gas is 3m 3 / h to 10m 3 / h.
[0047] In this embodiment, the process parameters of the first ventilation stage include: the power output range of the power supply is 50 kW to 60 kW, the gas pressure range of the reaction chamber is 50 kPa to 80 kPa, the flow rate range of the first gas is 7 m / s. 3 / h to 8m 3 / h.
[0048] Please continue to refer to Figure 1 and Figure 2 After the first ventilation, the second ventilation is performed, and the first gas is continuously introduced into the plasma generating chamber 201, and the reaction gas is introduced into the plasma generating chamber 201 at the same time, and a radio frequency plasma power source is used to dissociate the first gas and the reaction gas to form a mixed gas plasma 204.
[0049] Specifically, in the second ventilation stage, the flow rate of the first gas in the main air inlet 202 remains unchanged, the first gas is introduced from the side air inlet 203 at a set reduced speed, and the reaction gas is introduced from the side air inlet 203 at the same time.
[0050] Through the second ventilation stage, the first gas introduced from the side gas inlet 203 is slowly replaced by the reaction gas, and a mixed ion gas of the first gas and the reaction gas is established in the plasma generating chamber 201 .
[0051] Through the above two-step ventilation, the performance of the obtained mixed gas ion is stabilized, which is beneficial to control the subsequent reaction and further obtain a ceramic powder product with uniform particle size.
[0052] In this embodiment, the reaction gas includes oxygen. In this embodiment, through the second ventilation stage, a mixed gas plasma 204 of argon and oxygen is established in the plasma generating chamber 201 .
[0053] In the mixed gas plasma 204, the volume ratio of oxygen to the total gas volume ranges from 5% to 85%. Controlling the content of oxygen plasma is beneficial to controlling the reaction process rate and preventing the stoichiometric ratio of the generated ceramic powder components from deviating from the target.
[0054] In this embodiment, in the mixed gas plasma 204 , the volume of oxygen accounts for 20% to 60% of the total gas volume.
[0055] The process parameters of the second ventilation stage include: the power output range of the power supply is 40kW to 100kW, the gas pressure range of the reaction chamber is 80kPa to 110kPa, the first gas flow range is 3m 3 / h to 4m 3 / h, the flow range of the reaction gas is 2m 3 / h to 6m 3 / h.
[0056] In this embodiment, the process parameters of the second ventilation stage include: the power output range of the power supply is 40kW to 100kW, the gas pressure range of the reaction chamber is 80kPa to 100kPa, the first gas flow range is 3m 3 / h to 4m 3 / h, the flow range of the reaction gas is 3m 3 / h to 5m 3 / h.
[0057] Controlling the output power range of the power supply within 40 kW to 100 kW is beneficial to controlling the energy density of the plasma within a reasonable range and preventing different types of metal atoms from volatilizing or agglomerating in the plasma torch.
[0058] The gas source purity range of the mixed gas plasma is greater than or equal to 99.999%. The gas source of the mixed gas plasma includes the first gas and the reaction gas, and improving the gas source purity of the plasma is conducive to improving the purity of the ceramic powder product finally obtained.
[0059] Please continue to refer to Figure 1 , providing a solid raw material 205, wherein the solid raw material 205 includes two or more elemental metals.
[0060] The solid raw material 205 includes metal aluminum and metal magnesium. In this embodiment, the solid raw material 205 is an aluminum-magnesium alloy.
[0061] The molar ratio of aluminum to magnesium in the solid raw material 205 ranges from 1:1.81 to 1:2.17. In this embodiment, the molar ratio of aluminum to magnesium in the aluminum-magnesium alloy is 1:2.
[0062] In this embodiment, the ceramic powder obtained subsequently is magnesium aluminum spinel powder, whose chemical formula is MgAl2O4. By setting the molar ratio between each elemental metal in the solid raw material to be consistent with the molar ratio between each metal element in the target ceramic powder, the target ceramic powder with standard stoichiometry can be obtained, which is beneficial to improve the uniformity of the chemical composition of the ceramic powder.
[0063] The solid raw material may be in the form of powder, filament, wire, rod, or tube. In this embodiment, the solid raw material is wire.
[0064] The purity of the solid raw material is greater than or equal to 99.999%. Improving the purity of the raw material is conducive to improving the purity of the ceramic powder product finally obtained.
[0065] Please continue to refer to Figure 1and Figure 2 After the mixed gas plasma is formed, the solid raw material is sent to the plasma generating chamber 201, the solid raw material 205 is gasified in the plasma generating chamber 201 to form a gaseous raw material, and the gaseous raw material reacts with the dissociated reaction gas in the reaction chamber to generate a process product 208.
[0066] A radio frequency plasma power source is used to generate high-temperature plasma, and there is no secondary pollution of the electrode. The radio frequency plasma flame can fully heat the raw materials and the atmosphere in the reaction chamber is controllable, which is beneficial to improving the uniformity and purity of the product. The reaction gas is dissociated as plasma to provide a reaction heat source, and also as a product of the reaction gas and the raw material reaction to form the process. The process is simple and there are no by-products.
[0067] Specifically, since the temperature of the thermal plasma flame is as high as 10,000°C, the magnesium-aluminum alloy raw materials can be instantly melted and vaporized at such a high temperature, wherein the aluminum can not only be instantly oxidized, but also the oxidation reaction of the aluminum will not be prevented from further proceeding due to the formation of a solid oxide film, which is beneficial to improving the production efficiency and product quality of the product.
[0068] The method of feeding the solid raw material 205 into the plasma generating chamber includes: adding the solid raw material 205 from the outside of the plasma generating chamber 201 to the inside of the plasma generating chamber 201 through a feeding device or pre-setting the solid raw material 205 in the plasma generating chamber 201 .
[0069] In this embodiment, the top wall of the plasma generating chamber 201 has a feed port (not shown in the figure), and the aluminum-magnesium alloy wire is added into the interior of the plasma generating chamber 201 through the feed port.
[0070] The solid raw material 205 is delivered to the plasma generating chamber at a speed of 1 kg / h to 15 kg / h. In this embodiment, the solid raw material 205 is delivered to the plasma generating chamber at a speed of 2 kg / h to 8 kg / h.
[0071] Please continue to refer to Figure 1 and Figure 2 , by condensing the process product, ceramic powder is obtained.
[0072] In this embodiment, the method for condensing the process product includes: setting a plurality of condensation gas inlets (not shown in the figure) on the side wall of the reaction chamber, the plurality of condensation gas inlets are located below the plasma generating chamber 201 and are evenly arranged around the central axis of the reaction chamber; introducing condensation gas from the plurality of condensation gas inlets, and the condensation gas is blown toward the process product.
[0073] In this embodiment, the condensed gas includes nitrogen.
[0074] In this embodiment, the flow rate range of the condensed gas is 3m 3 / h to 8m 3 / h.
[0075] The material of the ceramic powder is aluminum magnesium spinel.
[0076] The ceramic powder is spherical powder.
[0077] The purity of the ceramic powder is greater than or equal to 99.999%, except for magnesium and aluminum. This means that the obtained ceramic powder product may contain magnesium and aluminum, and after removing magnesium and aluminum, the content of aluminum-magnesium spinel in the ceramic powder is greater than or equal to 99.999%.
[0078] The particle size distribution of the ceramic powder: D50 ranges from 20 nanometers to 300 nanometers, wherein the ratio of D90 to D50 is less than 3, and the ratio of D10 to D50 is greater than 0.3. D represents the diameter of the powder particles, D50 represents the diameter at the cumulative 50% point, D10 represents the diameter at the cumulative 10% point, and D90 represents the diameter at the cumulative 90% point. In this embodiment, the obtained ceramic powder particle size: D50 is 100 nanometers, D90 is less than 300 nanometers, and D10 is greater than 30 nanometers.
[0079] The aluminum-magnesium spinel ceramic powder has the characteristics of high purity, small particle size and narrow particle size distribution. The aluminum-magnesium spinel ceramic powder is used to prepare aluminum-magnesium spinel ceramics, which can improve the sintering density, thermal conductivity and light transmittance of the aluminum-magnesium spinel ceramics and can significantly reduce the sintering temperature of the magnesium-aluminum spinel ceramics.
[0080] Although the present invention is disclosed as above, the present invention is not limited thereto. Any person skilled in the art can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the protection scope of the present invention shall be subject to the scope defined by the claims.
Claims
1. A method for preparing ceramic powder, It is characterized in that include: A plasma device is provided, the plasma device comprising: a radio frequency plasma power supply, a reaction chamber, and a plasma generating chamber located at the top of the reaction chamber, wherein the plasma generating chamber is in communication with the reaction chamber, the plasma generating chamber has a main gas inlet and a side gas inlet, and the side gas inlet is located at the edge of the plasma generating chamber relative to the main gas inlet; Performing a first ventilation, introducing a first gas into the plasma generating chamber from the main gas inlet and the side gas inlet, and dissociating the first gas using a radio frequency plasma power supply; After the first ventilation, the second ventilation is performed, the first gas is continuously introduced into the plasma generating chamber, the flow rate of the first gas in the main gas inlet remains unchanged, the first gas is introduced from the side gas inlet at a set reduced speed, and at the same time, a reaction gas is introduced into the plasma generating chamber from the side gas inlet, and a radio frequency plasma power source is used to dissociate the first gas and the reaction gas to form a mixed gas plasma; Providing a solid raw material, wherein the solid raw material includes two or more elemental metals; After the mixed gas plasma is formed, a solid raw material is sent to the plasma generating chamber, the solid raw material is vaporized in the plasma generating chamber to form a gaseous raw material, and the gaseous raw material reacts with the dissociated reaction gas in the reaction chamber to generate a process product; By condensing the process product, a ceramic powder is obtained, wherein the particle size distribution of the ceramic powder is as follows: D50 ranges from 20 nanometers to 300 nanometers, wherein the ratio of D90 to D50 is less than 3, and the ratio of D10 to D50 is greater than 0.
3.
2. The method for preparing ceramic powder according to claim 1, It is characterized in that The process parameters of the first ventilation stage include: the power output range of the power supply is 30 kW to 60 kW, the gas pressure range of the reaction chamber is 50 kPa to 80 kPa, the flow rate range of the first gas is 3 m / s 3 / h to 10 m 3 / h; the process parameters of the second ventilation stage include: the power output range of the power supply is 40 kW to 100 kW, the gas pressure range of the reaction chamber is 80 kPa to 110 kPa, the first gas flow range is 3 m 3 / h to 4 m 3 / h, the flow range of the reaction gas is 2 m 3 / h to 6 m 3 / h.
3. The method for preparing ceramic powder according to claim 1, It is characterized in that The first gas includes argon, and the reaction gas includes oxygen.
4. The method for preparing ceramic powder according to claim 3, It is characterized in that In the mixed gas plasma, the volume of oxygen accounts for a proportion of the total gas volume in a range of 5% to 85%.
5. The method for preparing ceramic powder according to claim 1, It is characterized in that The solid raw materials include metal aluminum and metal magnesium.
6. The method for preparing ceramic powder according to claim 5, It is characterized in that The molar ratio of aluminum element to magnesium element in the solid raw material ranges from 1:1.81 to 1:2.
17.
7. The method for preparing ceramic powder according to claim 5, It is characterized in that The solid raw material may be in the form of one or more of powder, wire, rod, and tube.
8. The method for preparing ceramic powder according to claim 5, It is characterized in that The solid raw material is aluminum-magnesium alloy.
9. The method for preparing ceramic powder according to claim 5, It is characterized in that The material of the ceramic powder is aluminum-magnesium spinel; the ceramic powder is spherical powder; except for magnesium and aluminum metals, the purity of the ceramic powder is greater than or equal to 99.999%.
10. The method for preparing ceramic powder according to claim 1, It is characterized in that The solid raw material is fed into the plasma generation chamber at a rate of 1 kg / h to 15 kg / h.
11. The method for preparing ceramic powder according to claim 1, It is characterized in that The purity of the solid raw material is greater than or equal to 99.999%.
12. The method for preparing ceramic powder according to claim 1, It is characterized in that The method of feeding the solid raw material into the plasma generating chamber comprises: adding the solid raw material from the outside of the plasma generating chamber to the inside of the plasma generating chamber through a feeding device or pre-setting the solid raw material in the plasma generating chamber.
13. The method for preparing ceramic powder according to claim 1, It is characterized in that The gas source purity range of the mixed gas plasma is greater than or equal to 99.999%.