A method for preparing high-temperature nylon prepolymer with stable and controllable molecular weight
By using 3,4-perylene dicarboxylic acid to adjust the exchange rate of monomer amide and controlling the displacement during the prepolymerization stage of high-temperature nylon, the problem of unstable quality of existing high-temperature nylon products is solved, and the stability of the prepolymer molecular weight is achieved and The parallelism of multiple batches of experiments improves the stability of high-temperature nylon production and the quality of the final product.
Patent Information
- Application Number
- CN202310001881.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-01-03
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2043-01-03
AI Technical Summary
The quality of existing high-temperature nylon products is unstable, mainly due to the difficulty in controlling the high-temperature and high-pressure process in the prepolymerization stage, resulting in a large molecular weight distribution width, which affects the stability of the final product.
Through the principle of reaction kinetics, 3,4-perylene dicarboxylic acid is used as a molecular weight regulator to control the exchange rate of monomer amides, reduce the molecular weight distribution width, and stabilize the molecular weight of the prepolymer by precisely controlling the displacement, ensuring the subsequent polycondensation product quality.
The stability of the molecular weight of the prepolymer and the parallelism of multiple batches of experiments are achieved, and the stability of high-temperature nylon production and the quality of the final product are improved.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of materials and is a method for preparing a high-temperature nylon prepolymer with stable and controllable molecular weight. Background Art
[0002] High temperature nylon is a kind of special nylon. Most of the high temperature nylon is polymerized by aromatic diacids and aliphatic diamines, and a small amount is polymerized by aromatic diacids and aromatic diamines. High temperature nylon not only has good mechanical properties and heat resistance, but also has excellent properties such as wear resistance, solvent resistance, and corrosion resistance. Except for fully aromatic nylon, most high temperature nylons have very good processability. The most important thing is its excellent thermal stability, which is mainly used in the electronic and electrical fields and the automotive field. With the rapid development of lightweight automobiles and the electronics industry, the demand for high temperature nylon is growing. However, most of the industrialized high temperature nylon products on the market are in the hands of foreign companies. Although some domestic companies have successfully built industrialized equipment for high temperature nylon, the product quality is unstable, which limits the application of domestic high temperature nylon in the market.
[0003] After research, it was found that high-temperature nylon has more polymerization steps, and the polymerization temperature and polymerization pressure are relatively high, so the polymerization process is difficult to control. In particular, the prepolymerization stage involves high temperature and high pressure, and the parameters are extremely difficult to control. The stability of the prepolymer product will directly affect the stability of the final product quality, so stable prepolymer quality is conducive to the stability of high-temperature nylon production. Summary of the invention
[0004] In view of the deficiencies in the prior art, the present invention provides a method for preparing a high-temperature nylon prepolymer with a stable and controllable molecular weight.
[0005] The present invention improves the steric hindrance of the end-capping agent through the principle of reaction kinetics, makes it lag behind the monomer in participating in the reaction, ensures that the monomer has sufficient amide exchange rate, reduces the molecular weight distribution width, reduces the fluctuation of the molecular weight of the prepolymer, and then controls the molecular weight of the prepolymer by accurately controlling the displacement. The present invention can effectively and stably control the molecular weight of the prepolymer, which is beneficial to the quality and index stability of the final product after polycondensation.
[0006] The method provided by the invention is not only applicable to high-temperature nylon, but also applicable to the polymerization of other types of nylon.
[0007] The technical solution of the present invention is as follows:
[0008] A method for preparing a high-temperature nylon prepolymer with stable and controllable molecular weight comprises the following steps:
[0009] (1) 3,4-perylene dicarboxylic acid n-butyl ester is acidified, separated and dried to obtain 3,4-perylene dicarboxylic acid as a molecular weight regulator.
[0010] (2) adding high-temperature nylon monomer, molecular weight regulator, nucleating agent and deionized water of equal mass to the high-temperature nylon monomer into a salt-forming reactor, and replacing the reactor with inert gas; wherein the molecular weight regulator determines the molecular weight of the post-condensation product, and its amount can be determined according to the desired molecular weight of the post-condensation product.
[0011] (3) The salt-forming reactor is sealed and heated to 90-150° C., and the pressure is maintained at a stirring speed of 10-100 r / min for 1-3 hours to form a nylon salt solution.
[0012] (4) The nylon salt solution is transferred to the prepolymerization reactor through a filter, and the reactor is replaced with inert gas. After the replacement is completed, the reactor is heated to 200-280° C. and the pressure is maintained for 0.5-2 hours to carry out the prepolymerization reaction. After the reaction is completed, the water vapor in the reactor is discharged (the discharged water vapor is introduced into a condenser for condensation and collection and accurate measurement), and the drainage volume is monitored in real time. When the drainage volume reaches 0-95% of the total water input, the drainage is stopped, and the temperature and pressure are maintained for 1-4 hours. The prepolymer is discharged and the molecular weight of the prepolymer is tested.
[0013] Furthermore, concentrated hydrochloric acid is used for acidification in step 1.
[0014] Furthermore, the high temperature nylon monomer in step 2 is a mixture of an organic diacid and an organic diamine in a molar ratio of 1:1;
[0015] Further, the organic diacid is terephthalic acid, or a mixture of terephthalic acid and a dibasic acid;
[0016] The dibasic acid includes at least one of glutaric acid, adipic acid, sebacic acid, and dodecanedioic acid;
[0017] Furthermore, the organic diamine includes but is not limited to butanediamine, pentanediamine, hexamethylenediamine and the like.
[0018] Furthermore, the post-condensation product is a high-temperature nylon final polymer formed by further polycondensation of the prepolymer.
[0019] Furthermore, the nucleating agent in step 2 is calcium stearate, and the amount used is 0.1-0.5% of the total mass of the high-temperature nylon monomer.
[0020] Furthermore, the inert gas in step 2 is nitrogen.
[0021] Furthermore, the salt formation temperature in step 3 is preferably 120-140°C.
[0022] Furthermore, the stirring speed in step 3 is preferably 50 r / min.
[0023] Furthermore, the reaction time in step 3 is preferably 1-2 h.
[0024] Furthermore, the inert gas in step 4 is nitrogen.
[0025] Furthermore, the prepolymerization temperature in step 4 is preferably 250°C.
[0026] Furthermore, the reaction time in step 4 is preferably 2-3 h.
[0027] Furthermore, the water discharge in step 4 is 0%-95% of the total water input, preferably 40-80%.
[0028] The present invention has the following advantages:
[0029] 1. This method has a wide range of applications and is suitable for the preparation of prepolymers of various nylons.
[0030] 2. The nylon prepolymer prepared by this method has good relative molecular weight stability and good parallelism in multiple batch experiments. DETAILED DESCRIPTION
[0031] The present invention is further described below using nylon 6T / 66 prepolymer. The embodiments described in the present invention are only used to illustrate the present invention and do not limit the scope of the present invention.
[0032] [Example]
[0033] Homemade molecular weight regulator:
[0034] Referring to the paper "Synthesis and Properties of Perylene Dicarboxylate Compounds and Several Intramolecular Donor-Acceptor System Molecules", 3,4-perylene dicarboxylic acid n-butyl ester was synthesized; after acidification with hydrochloric acid, extraction separation and drying, 3,4-perylene dicarboxylic acid was obtained.
[0035] Embodiment 1
[0036] 913.7 g of terephthalic acid, 657.6 g of adipic acid, 1162.0 g of hexamethylenediamine, 13.6 g of calcium stearate, 13.6 g of a molecular weight regulator and 2733.3 g of water were added to a salt-forming reactor, the reactor was purged with nitrogen, the temperature was raised to 120° C. in a sealed state, and the reaction was carried out at a stirring speed of 90 r / min for 2 h to obtain a nylon salt solution;
[0037] The nylon salt solution is transferred to the prepolymerization reactor through a filter, and the reactor is replaced with nitrogen. After the replacement is completed, the reactor is heated to 250°C and the pressure is maintained for 1 hour for prepolymerization. After the reaction is completed, the water vapor in the reactor is discharged (the discharged water vapor is introduced into a condenser for condensation, collection and accurate measurement), and the drainage volume is monitored in real time. When the drainage volume reaches 80% of the total water input, the drainage is stopped, and the temperature and pressure are maintained for 2 hours. The prepolymer is discharged and the molecular weight of the prepolymer is tested.
[0038] The above experimental process was repeated 5 times as a reference for product stability, and the obtained product molecular weight is shown in Table 1.
[0039] Table 1
[0040] Displacement 80% 80% 80% 80% 80% 80% Molecular weight 3103 3127 3177 3107 3098 3149
[0041] Comparative Example 1
[0042] 913.7 g of terephthalic acid, 657.6 g of adipic acid, 1162.0 g of hexamethylenediamine, 13.6 g of calcium stearate, 13.6 g of a molecular weight regulator and 2733.3 g of water were added to a salt-forming reactor, the reactor was replaced with inert gas nitrogen, the temperature was raised to 120° C. in a sealed state, and the reaction was carried out at a stirring speed of 90 r / min for 2 h to obtain a nylon salt solution;
[0043] The nylon salt solution was transferred to the prepolymerization reactor through a filter, and the reactor was replaced with nitrogen. After the replacement was completed, the reactor was heated to 250°C and the pressure was maintained for 1 hour for prepolymerization. After the reaction was completed, the excess pressure was released, and the pressure in the reactor was reduced to 2.8MPa, and then the temperature and pressure were maintained for 2 hours (if the pressure exceeded 2.8MPa during the temperature and pressure maintenance process, the excess pressure was released to 2.8MPa), and the prepolymer was obtained by discharging the material, and the molecular weight of the prepolymer was tested.
[0044] The above experimental process was repeated 5 times as a reference for product stability comparison, and the obtained product molecular weight is shown in Table 2.
[0045] Table 2
[0046] pressure 2.8MPa 2.8MPa 2.8MPa 2.8MPa 2.8MPa 2.8MPa Molecular weight 3407 3074 2877 3209 3704 3200
[0047] Comparative Example II
[0048] 913.7 g of terephthalic acid, 657.6 g of adipic acid, 1162.0 g of hexamethylenediamine, 13.6 g of calcium stearate, an equal mole of adipic acid as a molecular weight regulator and 2733.3 g of water were added to a salt-forming reactor, the reactor was purged with nitrogen, the temperature was raised to 120° C. in a sealed state, and the reaction was carried out at a stirring speed of 90 r / min for 2 h to obtain a nylon salt solution;
[0049] The nylon salt solution is transferred to the prepolymerization reactor through a filter, and the reactor is replaced with nitrogen. After the replacement is completed, the reactor is heated to 250°C and the pressure is maintained for 1 hour for prepolymerization. After the reaction is completed, the water vapor in the reactor is discharged (the discharged water vapor is introduced into a condenser for condensation, collection and accurate measurement), and the drainage volume is monitored in real time. When the drainage volume reaches 80% of the total water input, the drainage is stopped, and the temperature and pressure are maintained for 2 hours. The prepolymer is discharged and the molecular weight of the prepolymer is tested.
[0050] The above experimental process was repeated 5 times as a reference for product stability, and the obtained product molecular weight is shown in Table 3.
[0051] Table 3
[0052] Displacement 80% 80% 80% 80% 80% 80% Molecular weight 3022 3498 3305 2987 3201 3199
[0053] Example II:
[0054] 913.7 g of terephthalic acid, 657.6 g of adipic acid, 1162.0 g of hexamethylenediamine, 13.6 g of calcium stearate, 13.6 g of a molecular weight regulator and 2733.3 g of water were added to a salt-forming reactor, the reactor was purged with nitrogen, the temperature was raised to 120° C. in a sealed state, and the reaction was carried out at a stirring speed of 50 r / min for 2 h to obtain a nylon salt solution;
[0055] The nylon salt solution is transferred to the prepolymerization reactor through a filter, and the reactor is replaced with inert gas nitrogen. After the replacement is completed, the reactor is heated to 250°C and the pressure is maintained for 1 hour for prepolymerization. After the reaction is completed, the water vapor in the reactor is discharged (the discharged water vapor is introduced into the condenser for condensation and collection and accurate measurement), and the drainage volume is monitored in real time. When the drainage volume reaches 80%, 70%, 60%, 50%, and 40% of the total water input, the drainage is stopped, and the temperature and pressure are maintained for 2 hours. The prepolymer is discharged and the molecular weight of the prepolymer is tested. The molecular weight of the product at different drainage volumes is shown in Table 4.
[0056] Table 4
[0057] Displacement 40% 50% 60% 70% 80% Molecular weight 1100 1400 2057 2487 3149
[0058] Comparison between Example I and Comparative Example I shows that the prepolymer obtained by controlling the displacement has better stability and smaller fluctuation between batches. Comparison between Example I and Comparative Example II shows that the prepolymer prepared by using 3,4-perylene dicarboxylic acid as a molecular weight regulator has smaller molecular weight fluctuation between batches and stronger stability.
[0059] The results of Example II show that the molecular weight of the prepolymer can be effectively and stably controlled by the present invention, and the molecular weight distribution and molecular weight of the prepolymer can be effectively controlled by making a self-made molecular weight regulator and controlling the drainage amount, which is beneficial to the quality and index stability of the final product after post-condensation.
Claims
1. A method for preparing a high-temperature nylon prepolymer with a stable and controllable molecular weight, comprising the following steps: (1) adding a high temperature nylon monomer, a molecular weight regulator 3,4-perylene dicarboxylic acid, a nucleating agent and deionized water into a salt-forming reactor, and replacing the reactor with an inert gas; (2) The salt-forming reaction kettle is sealed and heated to 90-150° C., and the pressure is maintained at a certain stirring speed to react to form a nylon salt solution; (3) The nylon salt solution is transferred to a prepolymerization reactor, and the reactor is replaced with an inert gas. After the replacement is completed, the reactor is heated to 200-280° C. and the prepolymerization reaction is carried out under pressure. After the reaction is completed, the water vapor in the reactor is released, and the drainage volume is monitored in real time. When the drainage volume reaches 40-95% of the total water input, the drainage is stopped, the temperature and pressure are maintained, and the prepolymer is discharged.
2. The method according to claim 1, characterized in that: The high temperature nylon monomer is a mixture of organic diacid and organic diamine in equal molar ratios.
3. The method according to claim 2, characterized in that: The organic diacid is terephthalic acid, or a mixture of terephthalic acid and a dibasic acid; The dibasic acid includes at least one of glutaric acid, adipic acid, sebacic acid, and dodecanedioic acid; The organic diamine includes at least one of butanediamine, pentanediamine and hexamethylenediamine.
4. The method according to any one of claims 1 to 3, characterized in that: In step (1), the deionized water and the high temperature nylon monomer are of equal mass.
5. The method according to any one of claims 1 to 3, characterized in that: The nucleating agent is calcium stearate.
6. The method according to claim 5, characterized in that The amount of the nucleating agent used is 0.1-0.5% of the total mass of the high-temperature nylon monomer.
7. The method according to claim 1, characterized in that: The inert gas is nitrogen.
8. The method according to claim 1, characterized in that: The rotation speed of step (2) is 10 to 100 r / min, and the pressure-maintaining reaction time is 1 to 3 hours.
9. The method according to claim 1, characterized in that: In step (3), the holding time of the prepolymerization reaction is 0.5 to 2 hours; and the holding time of the heat preservation and pressure preservation after stopping the drainage is 1 to 4 hours.
10. The method according to claim 1, characterized in that: In step (3), the exhausted water vapor is introduced into a condensation tank for condensation, collection and precise measurement.