Polyoxymethylene composition and method for preparing material containing the same

Through the synergistic effect of the composite antioxidant system and formic acid absorber, combining small molecule and polymer formaldehyde absorber, a low formaldehyde release polyformaldehyde composition was prepared, which solved the problem of large amount of small molecule substances in polyformaldehyde materials and improved the Mechanical and environmentally friendly properties of materials.

CN116199998BActive Publication Date: 2024-12-03CHINA ENERGY GRP NINGXIA COAL IND CO LTD +1
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
CN202310212488.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-07
Publication Date
2024-12-03
Estimated Expiration
2043-03-07

AI Technical Summary

Technical Problem

The existing polyformaldehyde materials have large release amounts of small molecules, which are difficult to meet stricter environmental protection standards, especially in applications in automotive interior parts, home appliances, bathrooms and other fields.

Method used

The synergistic effects of composite antioxidant system, formaldehyde absorption system, formic acid absorber, lubricant and crystallization nucleating agent are adopted, including small molecule and polymer formaldehyde absorber, and are melted, kneaded and granulated through a twin-screw extruder. Polyformaldehyde compositions with low formaldehyde release were prepared.

Benefits of technology

It significantly reduces the formaldehyde content and release amount in polyformaldehyde resin, improves the mechanical properties of the material and the stability of small-molecular substances, and is suitable for stricter environmental protection standards.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention provides a method for preparing a polyoxymethylene composition and a material containing the same. The composition comprises: by weight, 100 parts of polyoxymethylene resin, 0.04-2 parts of formaldehyde absorbent, 0.20-1 parts of antioxidant, 0.02-1 parts of formic acid absorbent, 0.05-1 parts of lubricant and 0.02-0.5 parts of crystal nucleating agent, the formaldehyde absorbent comprises a small molecule formaldehyde absorbent and a polymer formaldehyde absorbent; wherein the small molecule formaldehyde absorbent comprises any one or more of melamine and a derivative of melamine; and the polymer formaldehyde absorbent is a copolyamide resin containing a hydrazide end group. The polyoxymethylene composition is coupled by a composite antioxidant system, a formaldehyde absorption system, a formic acid absorbent, a lubricant and a crystal nucleating agent, wherein the formaldehyde absorption system comprises a small molecule formaldehyde absorbent and a polymer formaldehyde absorbent, and has better formaldehyde absorption and fixing effects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polyoxymethylene materials, and in particular to a polyoxymethylene composition and a method for preparing a material containing the polyoxymethylene composition. Background Art

[0002] Polyoxymethylene (POM) is an engineering plastic with high crystallinity and high melting point. It is one of the five general-purpose engineering plastics. POM not only has excellent wear resistance, insulation and self-lubrication, but also has metal-like hardness and strength. It is known as "Dusteel" and "Saisteel".

[0003] VOC (Volatile Organic Compounds) of polymer materials refers to organic compounds that are easily volatile at room temperature, such as formaldehyde, benzene, etc. Polyoxymethylene also has the problem of VOC. The VOC in polyoxymethylene generally refers to the free formaldehyde released by it. In recent years, polyoxymethylene has been widely used in precision instruments, home building materials, automobiles, electronic equipment and other fields due to its excellent performance, such as door and window parts, pulleys, bearings, gears, door handles, dashboards, seat belt buckles, shock absorbers and electrical switches. However, with the introduction of environmental health standards for indoor and passenger cars, these products have increasingly stringent requirements for VOC release, so the requirements for free formaldehyde release of polyoxymethylene products are also becoming increasingly stringent. Generally speaking, only polyoxymethylene with extremely low formaldehyde release can meet the extremely low small molecule substance release standard.

[0004] In order to reduce the free formaldehyde in polyoxymethylene, the general method is to add formaldehyde absorbents to polyoxymethylene. The current patents disclosed include dicyandiamide, melamine, melamine derivatives, polyethylene polyamines, low molecular weight amides and hydrazides. The active hydrogen in the formaldehyde absorbent reacts with formaldehyde gas to absorb and fix formaldehyde. However, the effect of these formaldehyde absorbents in absorbing and fixing formaldehyde is very limited, and they cannot be used to prepare polyoxymethylene with extremely low small molecular weight release. In addition, these traditional formaldehyde absorbents also have many problems such as volatilization, migration, color change, and poor formaldehyde absorption efficiency.

[0005] At present, most polyformaldehyde manufacturers produce general-purpose polyformaldehyde and other types of special materials. For general-purpose polyformaldehyde, since its antioxidant is basically a single antioxidant 245, its oxidation induction period is short and its thermal stability is insufficient. In addition, its formaldehyde absorption only uses ordinary melamine as an absorbent, so the free formaldehyde content and unstable end group content are high. A large amount of harmful formaldehyde substances are easily released during the processing. Therefore, general-purpose polyformaldehyde products are difficult to be widely used in fields with higher requirements, such as automotive interiors, home appliances, and sanitary ware.

[0006] The existing polyformaldehyde technology involving low odor, low molecular weight substance release, and low VOC mainly involves adding antioxidants, formaldehyde absorbers, and lubricants to the polymerized polyformaldehyde base powder during the post-processing extrusion granulation process, and obtaining polyformaldehyde particles through extrusion granulation. For example, CN104004317A provides a production method for preparing low VOC by adding formaldehyde absorbers, formic acid absorbers, antioxidants, and devolatilizers to polyformaldehyde; CN108440896A discloses a method for preparing low VOC polyformaldehyde by adding polyamide emulsion modified diatomaceous earth to polyformaldehyde base materials; CN113831681A discloses a method for preparing low-release polyformaldehyde by adding antioxidants, lubricants, stabilizers, and formaldehyde absorption aids. However, due to the failure to fully consider the coupling between different antioxidants, the selection of formaldehyde absorbers and formic acid absorbers is not stable and efficient enough, indicating that the effects of its antioxidant system, formaldehyde absorption system, and formic acid absorption system need to be improved. Summary of the invention

[0007] The main purpose of the present invention is to provide a polyoxymethylene composition, a polyoxymethylene material and a preparation method thereof, so as to solve the problem that the release amount of small molecule substances of polyoxymethylene in the prior art is too large.

[0008] In order to achieve the above-mentioned object, according to one aspect of the present invention, a polyoxymethylene composition is provided, which comprises: in parts by weight, 100 parts of polyoxymethylene resin, 0.04-2 parts of formaldehyde absorbent, 0.20-1 parts of antioxidant, 0.02-1 parts of formic acid absorbent, 0.05-1 parts of lubricant and 0.02-0.5 parts of crystallization nucleating agent, wherein the formaldehyde absorbent comprises a small molecule formaldehyde absorbent and a high molecular formaldehyde absorbent; wherein the small molecule formaldehyde absorbent comprises any one or more of melamine and its derivatives; and the high molecular formaldehyde absorbent is a copolyamide resin containing hydrazide end groups.

[0009] Furthermore, the content of the polymer formaldehyde absorbent is 0.02-1 parts by weight. Preferably, the particle size of the polymer formaldehyde absorbent is ≤55 μm. Preferably, the melting point of the polymer formaldehyde absorbent is greater than 140°C.

[0010] Furthermore, the composition also includes 0.01-2 parts by weight of a formaldehyde fixative, which is a low molecular weight polyester resin containing a hydrazide end group; preferably, the molecular weight of the formaldehyde fixative is 1000-5000 g / mol; preferably, the particle size of the formaldehyde fixative is less than or equal to 55 μm, and preferably, the melting point of the formaldehyde fixative is greater than 130°C.

[0011] Furthermore, the formic acid absorbent is a compound of the inorganic compound represented by Formula I and stearate.

[0012] Mg 1-x Al x (OH)2 An- x / n ·mH2O Formula I

[0013] In the formula, A n- It is an n-valent anion, n is an integer of 1-3, x=0.2-0.33, and m is 2-6;

[0014] Preferably, the particle size of the inorganic compound is less than or equal to 10 μm;

[0015] Preferably, the stearate is selected from any one or more of calcium stearate, barium stearate, zinc stearate and magnesium stearate;

[0016] Preferably, the weight ratio of the inorganic compound to the stearate is 4:6 to 6:4.

[0017] Further, the antioxidant is a composite antioxidant; preferably, the composite antioxidant includes a first antioxidant, a second antioxidant and a third antioxidant, the first antioxidant includes triethylene glycol bis-β-(3-tert-butyl-4-hydroxy-5-methylphenyl) propionate, the second antioxidant includes any one or more of N,N-bis-(3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionyl) hexanediamine, tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate] pentaerythritol ester and β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate n-octadecyl alcohol ester, and the third antioxidant includes any one or more of tris(2,4-di-tert-butylphenyl) phosphite, dioctadecyl pentaerythritol diphosphite and bis(2,4-di-tert-butylphenol) pentaerythritol diphosphite;

[0018] Preferably, the weight ratio of the first antioxidant, the second antioxidant and the third antioxidant is 1:(0.25-1.5):(0.25-2.5).

[0019] Further, the melt index of the polyoxymethylene resin is 1.0-550.0 g / 10 min;

[0020] And / or, the lubricant includes any one or more of N,N-ethylene bisstearamide and glyceryl monostearate.

[0021] Furthermore, the crystal nucleating agent is any one or more of fumed silica, talc, and kaolin;

[0022] Preferably, the particle size of the fumed silica is no greater than 100 nm;

[0023] Preferably, the particle size of talc is no greater than 8 μm;

[0024] Preferably, the particle size of kaolin is no greater than 8 μm.

[0025] According to another aspect of the present application, a method for preparing a polyformaldehyde material is provided, the method comprising: adding any of the above-mentioned polyformaldehyde compositions into a blender for uniform premixing, and using a twin-screw extruder for melting, mixing, and granulation to obtain the polyformaldehyde material.

[0026] Furthermore, the temperature of each section of the extruder is 170-245° C., and the rotation speed of the twin-screw extruder is 20-600 r / min.

[0027] Furthermore, the aspect ratio of the twin-screw extruder is 25-70:1, and the vacuum degree of each exhaust section of the twin-screw extruder is ≤-0.06MPa during operation.

[0028] According to another aspect of the present application, a polyoxymethylene material is provided. The polyoxymethylene material is prepared from any one of the polyoxymethylene compositions described above, or is prepared by the preparation method described above.

[0029] By applying the technical solution of the present invention, the polyformaldehyde composition is coupled through a composite antioxidant system, a formaldehyde absorption system, a formic acid absorbent, a lubricant and a crystal nucleating agent, wherein the formaldehyde absorption system includes a small molecule formaldehyde absorbent and a polymer formaldehyde absorbent, and has better formaldehyde absorption and fixation effects than traditional general-purpose polyformaldehyde and other low-formaldehyde-releasing polyformaldehyde products; through the synergistic effect with the antioxidant, the formic acid absorbent, the lubricant and the crystal nucleating agent, the polyformaldehyde resin crystal morphology is effectively reduced, the mechanical properties of the polyformaldehyde material are improved, and less small molecule substances are released. In particular, the copolyamide resin polymer formaldehyde absorbent containing hydrazide end groups can effectively reduce the formaldehyde content in the POM resin, and the substance can effectively neutralize and adsorb the formaldehyde in the POM resin for a long time, and can play the role of a good formaldehyde absorbent. DETAILED DESCRIPTION

[0030] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present invention will be described in detail below in conjunction with the embodiments.

[0031] As analyzed in the background technology of the present application, the polyoxymethylene in the prior art has the problem of a relatively large release of small molecule substances. In order to solve this problem, the present application provides a polyoxymethylene composition and a method for preparing a material containing the same.

[0032] According to a typical embodiment of the present application, a polyformaldehyde composition is provided, which includes: in parts by weight, 100 parts of polyformaldehyde resin, 0.04-2 parts of formaldehyde absorber, 0.20-1 parts of antioxidant, 0.02-1 parts of formic acid absorber, 0.05-1 parts of lubricant and 0.02-0.5 parts of crystallization nucleating agent, the formaldehyde absorber includes a small molecule formaldehyde absorber and a polymer formaldehyde absorber; wherein the small molecule formaldehyde absorber includes any one or more of melamine and melamine derivatives; the polymer formaldehyde absorber is a copolyamide resin containing hydrazide end groups.

[0033] The polyformaldehyde composition of the present application is coupled by a composite antioxidant system, a formaldehyde absorption system, a formic acid absorbent, a lubricant and a crystal nucleating agent, wherein the formaldehyde absorption system includes a small molecule formaldehyde absorbent and a polymer formaldehyde absorbent, and has better formaldehyde absorption and fixation effects than traditional general-purpose polyformaldehyde and other low-formaldehyde-releasing polyformaldehyde products; through the synergistic effect with the antioxidant, the formic acid absorbent, the lubricant and the crystal nucleating agent, the crystalline morphology of the polyformaldehyde resin is effectively reduced, the mechanical properties of the polyformaldehyde material are improved, and the small molecule substances released are less. In particular, the copolyamide resin polymer formaldehyde absorbent containing hydrazide end groups can effectively reduce the formaldehyde content in the POM resin, and the substance can effectively neutralize and adsorb the formaldehyde in the POM resin for a long time, and can play the role of a good formaldehyde absorbent.

[0034] In some embodiments of the present application, the content of the polymer formaldehyde absorbent is 0.02-1 parts by weight, and correspondingly, the content of the small molecule formaldehyde absorbent is 0.02-1 parts by weight. The copolyamide resin containing hydrazide end groups is in powder form. Preferably, the particle size of the above-mentioned polymer formaldehyde absorbent is ≤55μm, which can make the powdered copolyamide resin and the polyformaldehyde powder fully mixed and melted synchronously in the extruder barrel. If the particle size is too large, the copolyamide resin cannot be fully mixed with the polyformaldehyde melt. Further, since the large particles of copolyamide cannot be fully melted with the polyformaldehyde, they will adhere to the filter screen of the extruder head, thereby clogging the filter screen and carbonizing, and finally causing the polyformaldehyde particles to have black spots or a high yellow index; and the copolyamide resin particle size is too large, which is not conducive to improving the absorption effect of formaldehyde. Preferably, the melting point of the polymer formaldehyde absorbent is greater than 140°C, which has a good absorption effect on formaldehyde, and is easy to melt synchronously with polyformaldehyde, which is beneficial to improve the comprehensive performance of polyformaldehyde.

[0035] In some preferred embodiments of the present application, the polyformaldehyde composition further comprises 0.01-2 parts by weight of a formaldehyde fixing agent, which is a low molecular weight polyester resin containing hydrazide end groups. The researchers of the present application unexpectedly found that the low molecular weight polyester resin containing hydrazide end groups has a better effect of absorbing formaldehyde than the copolyamide resin containing hydrazide end groups. Moreover, when the low molecular weight polyester resin containing hydrazide end groups is compounded with the copolyamide resin containing hydrazide end groups, it can produce a significant synergistic effect with certain specific combinations of composite formic acid absorbents and composite antioxidants, thereby greatly reducing the free formaldehyde content in the polyformaldehyde resin, and achieving unexpected technical effects. The low molecular weight polyester resin containing hydrazide end groups is in powder form. Preferably, the molecular weight of the formaldehyde fixing agent is 1000-5000 g / mol, which has a better fixing effect on formaldehyde; preferably, the particle size of the formaldehyde fixing agent is less than or equal to 55 μm, and preferably, the melting point of the formaldehyde fixing agent is greater than 130°C.

[0036] Since formic acid formed after the oxidation of trace formaldehyde in the production and processing of polyformaldehyde resin has an acidolysis effect on the polyformaldehyde resin, producing more low-molecular substances such as formaldehyde, a formic acid absorber is added to the polyformaldehyde composition of the present application. In some typical embodiments of the present application, the formic acid absorber is a composite of an inorganic compound shown in Formula I and a stearate. The above-mentioned low-molecular organic formic acid absorber is combined with hydrated magnesium aluminum carbonate to form a highly efficient two-component formic acid absorber, which further ensures that the polyformaldehyde resin achieves the purpose of extremely low release of small molecular substances during production and multiple processing.

[0037] Mg 1-x Al x (OH)2 A n- x / n ·mH2O Formula I

[0038] In the formula, A n- is an n-valent anion, exemplarily, A n- NO3 - 、CO3 2- 、SO4 2- , Cl - or a mixture thereof, n is an integer of 1-3, x=0.2-0.33, and m is 2-6. Exemplarily, the inorganic compound is selected from Mg 0.8 Al 0.2 (OH)2NO3·4.5H2O (x=0.20, n=0.20, m=4.5), Mg 0.75 Al 0.25 (OH)2(CO3)2·3.5H2O (x=0.25, n=0.125, m=3.5) and Mg 0 .67 Al 0 .33 (OH)2 (SO4 )6.6 ·2.5H2O (x=0.33, n=0.05, m=2.5). Preferably, the particle size of the inorganic compound is less than or equal to 10 μm;

[0039] The stearate includes but is not limited to any one or more of calcium stearate, barium stearate, zinc stearate and magnesium stearate. In some embodiments of the present application, the weight ratio of the inorganic compound to the stearate is 4:6 to 6:4.

[0040] The above-mentioned antioxidants can be selected from the prior art. In some embodiments of the present application, in order to further reduce the release of small molecules such as formaldehyde, the antioxidant is a composite antioxidant, that is, a combination of multiple antioxidants. The researchers of the present application found that the use of composite antioxidants can significantly reduce formaldehyde release.

[0041] In some typical embodiments of the present application, the composite antioxidant includes a first antioxidant, a second antioxidant and a third antioxidant, wherein the first antioxidant includes triethylene glycol bis-β-(3-tert-butyl-4-hydroxy-5-methylphenyl) propionate, the second antioxidant includes any one or more of N,N-bis-(3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionyl) hexanediamine, tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate] pentaerythritol ester and β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate n-octadecyl alcohol ester, and the third antioxidant includes any one or more of tris(2,4-di-tert-butylphenyl) phosphite, dioctadecyl pentaerythritol diphosphite and bis(2,4-di-tert-butylphenol) pentaerythritol diphosphite, which has a particularly significant effect on reducing the release of small molecules such as formaldehyde from the above-mentioned polyoxymethylene copolymer. Exemplarily, the composite antioxidant is triethylene glycol bis-β-(3-tert-butyl-4-hydroxy-5-methylphenyl) propionate / N,N-bis-(3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionyl) hexanediamine / tris(2,4-di-tert-butylphenyl) phosphite, triethylene glycol bis-β-(3-tert-butyl-4-hydroxy-5-methylphenyl) propionate / tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate] pentaerythritol / tris(2,4-di-tert-butylphenyl) phosphite. ester, triethylene glycol bis-β-(3-tert-butyl-4-hydroxy-5-methylphenyl) propionate / N,N-bis-(3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionyl) hexanediamine / dioctadecyl pentaerythritol diphosphite, triethylene glycol bis-β-(3-tert-butyl-4-hydroxy-5-methylphenyl) propionate / N,N-bis-(3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionyl) hexanediamine / bis(2,4-di-tert-butyl Phenol) Pentaerythritol diphosphite, Triethylene glycol bis-β-(3-tert-butyl-4-hydroxy-5-methylphenyl) propionate / β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate octadecyl alcohol ester / tris(2,4-di-tert-butylphenyl) phosphite, Triethylene glycol bis-β-(3-tert-butyl-4-hydroxy-5-methylphenyl) propionate / β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate octadecyl alcohol ester / dioctadecyl pentaerythritol diphosphite, Triethylene glycol bis-β-(3-tert-butyl-4-hydroxy-5-methylphenyl) propionate / β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate octadecyl alcohol ester / bis(2,4-di-tert-butylphenol) pentaerythritol diphosphite, triethylene glycol bis-β-(3-tert-butyl-4-hydroxy-5-methylphenyl) propionate / β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate octadecyl alcohol ester / bis(2,4-di-tert-butylphenol) pentaerythritol diphosphite.

[0042] In some embodiments, the weight ratio of the first antioxidant, the second antioxidant, and the third antioxidant is 1:(0.25-1.5:(0.25-2.5), such as a weight ratio of 1:1:1, 1:1:2, or 2:1:0.5.

[0043] The polyoxymethylene resin can be selected from the prior art. Preferably, the melt index of the polyoxymethylene resin is 1.0-550.0 g / 10min.

[0044] The lubricant can be selected from the prior art, such as any one or more of N,N-ethylene bisstearamide and glyceryl monostearate.

[0045] The above-mentioned crystal nucleating agent can be selected from the prior art. In some embodiments of the present application, the composite antioxidant, formic acid absorbent, formaldehyde absorbent and formaldehyde fixative of the present application are comprehensively considered to have an effect on the microstructure, crystal morphology and performance of polyformaldehyde. In some embodiments of the present application, the crystal nucleating agent is any one or more of fumed silica, talcum powder and kaolin, which can better adjust the size of polyformaldehyde crystals and improve mechanical properties. Preferably, the particle size of fumed silica is not more than 100nm, the particle size of talcum powder is not more than 8μm, and the particle size of kaolin is not more than 8μm.

[0046] According to another typical embodiment of the present application, a method for preparing a polyformaldehyde material is provided, wherein any one of the above-mentioned polyformaldehyde compositions is added to a mixer and premixed evenly, and then a twin-screw extruder is used for melting, mixing, and granulation to obtain the polyformaldehyde material.

[0047] The above preparation method couples a composite antioxidant system, a formaldehyde absorption system, a formic acid absorbent, a lubricant and a crystal nucleating agent, wherein the formaldehyde absorption system includes a small molecule formaldehyde absorbent and a polymer formaldehyde absorbent, and has better formaldehyde absorption and fixation effects than traditional general-purpose polyformaldehyde and other low-formaldehyde-releasing polyformaldehyde products; through the synergistic effect with the antioxidant, the formic acid absorbent, the lubricant and the crystal nucleating agent, the crystalline morphology of the polyformaldehyde resin is effectively reduced, the mechanical properties of the polyformaldehyde material are improved, and less small molecule substances are released. In particular, the copolyamide resin polymer formaldehyde absorbent containing hydrazide end groups can effectively reduce the formaldehyde content in the POM resin, and the substance can effectively neutralize and adsorb the formaldehyde in the POM resin for a long time, and can play the role of a good formaldehyde absorbent. The preparation method is simple and easy to implement and easy to apply industrially.

[0048] In some embodiments of the present application, the temperature of each section of the extruder is 170-245° C., and the rotation speed of the twin-screw extruder is 20-600 r / min.

[0049] In some embodiments, the twin-screw extruder used is a large-capacity evaporation (multi-stage exhaust) devolatilization twin-screw unit. Preferably, the aspect ratio of the twin-screw extruder is 25-70:1, and the vacuum degree of each exhaust section of the twin-screw extruder during operation is ≤-0.06MPa.

[0050] According to another typical embodiment of the present application, a polyoxymethylene material is provided, which is prepared from any of the above polyoxymethylene compositions or prepared by the above preparation method. The polyoxymethylene material has good mechanical properties and a small release amount of small molecule substances.

[0051] The beneficial effects that can be achieved by the present application will be further illustrated below in combination with embodiments and comparative examples.

[0052] The polyoxymethylene raw materials used in the examples and comparative examples of the present application are produced by the National Energy Ningxia Coal Industry Group.

[0053] Example 1

[0054] The polyoxymethylene composition ratio is as follows:

[0055] Copolymer polyoxymethylene resin: 100 parts, melt index 9.0g / 10min;

[0056] 0.2 parts of small molecule formaldehyde absorber, which is melamine;

[0057] 0.2 parts of polymer formaldehyde absorbent, composed of PA6 / PA1010 copolyamide resin containing hydrazide end groups, in powder form, with a particle size of 25 μm and a melting point of 160°C;

[0058] 0.2 parts of formaldehyde fixative, composed of low molecular weight polyester resin containing hydrazide end groups, with a molecular weight of 2000 g / mol, in powder form, a particle size of 30 μm, a melting point of 150°C, manufactured by Dongrui Chemical Company, model DR803PA;

[0059] 0.20 parts of composite antioxidant, the components are triethylene glycol bis-β-(3-tert-butyl-4-hydroxy-5-methylphenyl) propionate / N, N-bis-(3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionyl) hexanediamine / tris(2,4-di-tert-butylphenyl) phosphite, and the weight ratio of the three components is 1:1:1;

[0060] 0.2 parts of composite formic acid absorbent, composition: Mg6Al2(OH) 16 Compound of CO3·4H2O and zinc stearate, weight ratio of 1:1; Mg6Al2(OH) 16 The particle size of CO3·4H2O is 8 μm;

[0061] 0.1 part of lubricant, composed of N,N-ethylene bisstearamide;

[0062] 0.1 part of crystal nucleating agent, composed of fumed silica, with a particle size of 60 nm;

[0063] The above materials are added into a high-speed mixer and premixed uniformly, and then a twin-screw extruder is used for melting, mixing, extrusion and granulation to obtain a composition; the processing temperatures of each section of the extruder are 185°C, 195°C, 200°C, 210°C, 220°C, 225°C, 210°C, 200°C, 190°C, and the screw speed is 100r / min; the twin-screw extruder used is a large-capacity evaporation (multi-stage exhaust) devolatilization twin-screw unit with a length-to-diameter ratio of 65:1, and the vacuum degree of each exhaust section of the twin-screw extruder during operation is -0.08MPa.

[0064] Example 2

[0065] The polyoxymethylene composition ratio is as follows:

[0066] Copolymer polyoxymethylene resin: 100 parts, melt index 9.0g / 10min;

[0067] 0.2 parts of small molecule formaldehyde absorbent, which is a derivative of melamine, methyl cyanamide, produced by Hubei Fengcheng Chemical Co., Ltd.;

[0068] 0.3 parts of polymer formaldehyde absorbent, which is composed of PA6 / PA1010 copolyamide resin containing hydrazide end groups, in powder form, with a particle size of 25 μm and a melting point of 160°C;

[0069] 0.3 parts of formaldehyde fixative, which is a low molecular weight polyester resin containing hydrazide end groups, with a molecular weight of 1000 g / mol, in powder form, a particle size of 20 μm, and a melting point of 131°C. The manufacturer is Dongrui Chemical Company;

[0070] 0.20 parts of composite antioxidant, the ingredients are triethylene glycol bis-β-(3-tert-butyl-4-hydroxy-5-methylphenyl) propionate / pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate] / tris(2,4-di-tert-butylphenyl) phosphite, the weight ratio of the three components is 1:1:2;

[0071] 0.3 parts of composite formic acid absorbent, composition: Mg6Al2(OH) 16 A compound of CO3·4H2O and barium stearate, with a weight ratio of 1.2:1; Mg6Al2(OH) 16 The particle size of CO3·4H2O is 8 μm;

[0072] 0.1 part of lubricant, composed of N,N-ethylene bisstearamide;

[0073] 0.1 part of crystal nucleating agent, composed of talc powder, with a particle size of 5 μm;

[0074] The above materials are added into a high-speed mixer and premixed uniformly, and then a twin-screw extruder is used for melting, mixing, extrusion and granulation to obtain a composition; the processing temperatures of each section of the extruder are 185°C, 195°C, 200°C, 210°C, 220°C, 225°C, 210°C, 200°C, 190°C, and the screw speed is 100r / min; the twin-screw extruder used is a large-capacity evaporation (multi-stage exhaust) devolatilization twin-screw unit with a length-to-diameter ratio of 65:1, and the vacuum degree of each exhaust section of the twin-screw extruder during operation is -0.08MPa.

[0075] Example 3

[0076] The polyoxymethylene composition ratio is as follows:

[0077] Copolymer polyoxymethylene resin: 100 parts, melt index 9.0g / 10min;

[0078] 0.4 parts of small molecule formaldehyde absorber, which is melamine;

[0079] 0.4 parts of polymer formaldehyde absorbent, which is composed of PA6 / PA1010 copolyamide resin containing hydrazide end groups, in powder form, with a particle size of 25 μm and a melting point of 160°C;

[0080] 2.0 parts of formaldehyde fixative, which is a low molecular weight polyester resin containing hydrazide end groups, with a molecular weight of 5000 g / mol, in powder form, a particle size of 55 μm, and a melting point of 170°C. The manufacturer is Shanghai Zhenwei Composite Materials Co., Ltd.;

[0081] 0.30 parts of composite antioxidant, the ingredients are triethylene glycol bis-β-(3-tert-butyl-4-hydroxy-5-methylphenyl) propionate / N, N-bis-(3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionyl) hexanediamine / dioctadecyl pentaerythritol diphosphite, the weight ratio of the three components is 1:1:1;

[0082] 0.3 parts of composite formic acid absorbent, composition: Mg6Al2(OH) 16 Compound of CO3·4H2O and calcium stearate, weight ratio of 1.2:1; Mg6Al2(OH) 16 The particle size of CO3·4H2O is 8 μm;

[0083] 0.2 parts of lubricant, composed of N,N-ethylene bisstearamide;

[0084] 0.2 parts of crystal nucleating agent, composed of kaolin, with a particle size of 3 μm;

[0085] The above materials are added into a high-speed mixer and premixed uniformly, and then a twin-screw extruder is used for melting, mixing, extrusion and granulation to obtain a composition; the processing temperatures of each section of the extruder are 185°C, 195°C, 200°C, 210°C, 220°C, 225°C, 210°C, 200°C, 190°C, and the screw speed is 100r / min; the twin-screw extruder used is a large-capacity evaporation (multi-stage exhaust) devolatilization twin-screw unit with a length-to-diameter ratio of 65:1, and the vacuum degree of each exhaust section of the twin-screw extruder during operation is -0.08MPa.

[0086] Example 4

[0087] The polyoxymethylene composition ratio is as follows:

[0088] Copolymer polyoxymethylene resin: 100 parts, melt index 27.0g / 10min;

[0089] 0.5 parts of small molecule formaldehyde absorbent, which is a derivative of melamine, methyl cyanamide, produced by Hubei Fengcheng Chemical Co., Ltd.;

[0090] 0.5 parts of polymer formaldehyde absorbent, which is composed of PA6 / PA1010 copolyamide resin containing hydrazide end groups, in powder form, with a particle size of 25 μm and a melting point of 160°C;

[0091] 1.5 parts of formaldehyde fixative, which is a low molecular weight polyester resin containing hydrazide end groups, with a molecular weight of 3000 g / mol, in powder form, a particle size of 30 μm, and a melting point of 180°C. The manufacturer is Shanghai Zhenwei Composite Materials Co., Ltd.;

[0092] 0.40 parts of composite antioxidant, the components are triethylene glycol bis-β-(3-tert-butyl-4-hydroxy-5-methylphenyl) propionate / N, N-bis-(3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionyl) hexanediamine / tris(2,4-di-tert-butylphenyl) phosphite, the weight ratio of the three components is 1:1:1;

[0093] 0.3 parts of composite formic acid absorbent, composition: Mg6Al2(OH) 16 Compound of CO3·4H2O and magnesium stearate, weight ratio of 1.2:1; Mg6Al2(OH) 16 The particle size of CO3·4H2O is 8 μm;

[0094] 0.2 parts of lubricant, composed of glyceryl monostearate;

[0095] 0.4 parts of crystal nucleating agent, composed of fumed silica, with a particle size of 60 nm;

[0096] The above materials are added into a high-speed mixer and premixed uniformly, and then a twin-screw extruder is used for melting, mixing, extrusion and granulation to obtain a composition; the processing temperatures of each section of the extruder are 185°C, 195°C, 200°C, 210°C, 220°C, 225°C, 210°C, 200°C, 190°C, and the screw speed is 100r / min; the twin-screw extruder used is a large-capacity evaporation (multi-stage exhaust) devolatilization twin-screw unit with a length-to-diameter ratio of 65:1, and the vacuum degree of each exhaust section of the twin-screw extruder during operation is -0.08MPa.

[0097] Example 5

[0098] The polyoxymethylene composition ratio is as follows:

[0099] Copolymer polyoxymethylene resin: 100 parts, melt index 27.0g / 10min;

[0100] 0.6 parts of small molecule formaldehyde absorbent, which is a derivative of melamine, methyl cyanamide, produced by Hubei Fengcheng Chemical Co., Ltd.;

[0101] 0.6 parts of polymer formaldehyde absorbent, which is composed of PA6 / PA1010 copolyamide resin containing hydrazide end groups, in powder form, with a particle size of 25 μm and a melting point of 160°C;

[0102] 1.0 part of formaldehyde fixative, composed of low molecular weight polyester resin containing hydrazide end groups, with a molecular weight of 2000 g / mol, in powder form, a particle size of 30 μm, a melting point of 150°C, and produced by Dongrui Chemical Company;

[0103] 0.50 parts of composite antioxidant, the ingredients are triethylene glycol bis-β-(3-tert-butyl-4-hydroxy-5-methylphenyl) propionate / N, N-bis-(3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionyl) hexanediamine / bis(2,4-di-tert-butylphenol) pentaerythritol diphosphite, the weight ratio of the three components is 2:1:0.5;

[0104] 0.3 parts of composite formic acid absorbent, composition: Mg6Al2(OH) 16 SO4·4H2O and magnesium stearate compound, weight ratio of the two is 1.2:1; Mg6Al2(OH) 16 The particle size of SO4·4H2O is 6 μm;

[0105] 0.3 parts of lubricant, composed of N,N-ethylene bisstearamide;

[0106] 0.4 parts of crystal nucleating agent, composed of talc powder, with a particle size of 5 μm;

[0107] The above materials are added into a high-speed mixer and premixed uniformly, and then a twin-screw extruder is used for melting, mixing, extrusion and granulation to obtain a composition; the processing temperatures of each section of the extruder are 185°C, 195°C, 200°C, 210°C, 220°C, 225°C, 210°C, 200°C, 190°C, and the screw speed is 100r / min; the twin-screw extruder used is a large-capacity evaporation (multi-stage exhaust) devolatilization twin-screw unit with a length-to-diameter ratio of 65:1, and the vacuum degree of each exhaust section of the twin-screw extruder during operation is -0.08MPa.

[0108] Example 6

[0109] The polyoxymethylene composition ratio is as follows:

[0110] Copolymer polyoxymethylene resin: 100 parts, melt index 27.0g / 10min;

[0111] 0.7 parts of small molecule formaldehyde absorber, which is melamine;

[0112] 0.7 parts of polymer formaldehyde absorbent, which is composed of PA6 / PA1010 copolyamide resin containing hydrazide end groups, in powder form, with a particle size of 25 μm and a melting point of 160°C;

[0113] 0.7 parts of formaldehyde fixative, which is a low molecular weight polyester resin containing hydrazide end groups, with a molecular weight of 4300 g / mol, in powder form, a particle size of 5 μm, and a melting point of 190°C. The manufacturer is Shanghai Zhenwei Composite Materials Co., Ltd.;

[0114] 0.60 parts of composite antioxidant, the components are triethylene glycol bis-β-(3-tert-butyl-4-hydroxy-5-methylphenyl) propionate / β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate / tris(2,4-di-tert-butylphenyl) phosphite, and the weight ratio of the three components is 1:1:1;

[0115] 0.3 parts of composite formic acid absorbent, composition: Mg6Al2(OH) 16 SO4·4H2O and calcium stearate compound, the weight ratio of the two is 1:1; Mg6Al2(OH) 16 The particle size of SO4·4H2O is 6 μm;

[0116] 0.3 parts of lubricant, composed of glyceryl monostearate;

[0117] 0.4 parts of crystal nucleating agent, composed of kaolin, with a particle size of 3 μm;

[0118] The above materials are added into a high-speed mixer and premixed uniformly, and then a twin-screw extruder is used for melting, mixing, extrusion and granulation to obtain a composition; the processing temperatures of each section of the extruder are 185°C, 195°C, 200°C, 210°C, 220°C, 225°C, 210°C, 200°C, 190°C, and the screw speed is 100r / min; the twin-screw extruder used is a large-capacity evaporation (multi-stage exhaust) devolatilization twin-screw unit with a length-to-diameter ratio of 65:1, and the vacuum degree of each exhaust section of the twin-screw extruder during operation is -0.08MPa.

[0119] Example 7

[0120] The polyoxymethylene composition ratio is as follows:

[0121] Copolymer polyoxymethylene resin: 100 parts, melt index 27.0g / 10min;

[0122] 0.8 parts of small molecule formaldehyde absorber, which is a derivative of melamine;

[0123] 0.8 parts of polymer formaldehyde absorbent, composed of PA6 / PA1010 copolyamide resin containing hydrazide end groups, in powder form, with a particle size of 25 μm and a melting point of 160°C;

[0124] 0.05 parts of formaldehyde fixative, composed of low molecular weight polyester resin containing hydrazide end groups, with a molecular weight of 1100 g / mol, in powder form, with a particle size of 12 μm and a melting point of 155°C, produced by Dongrui Chemical Company;

[0125] 0.70 parts of composite antioxidant, the components are triethylene glycol bis-β-(3-tert-butyl-4-hydroxy-5-methylphenyl) propionate / β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate / bis(2,4-di-tert-butylphenol) pentaerythritol diphosphite, the weight ratio of the three components is 1:1:2;

[0126] 0.5 parts of composite formic acid absorbent, composition: Mg6Al2(OH) 16 SO4·4H2O and calcium stearate compound, the weight ratio of the two is 1:1; Mg6Al2(OH) 16 The particle size of SO4·4H2O is 6 μm;

[0127] 0.3 parts of lubricant, composed of N,N-ethylene bisstearamide;

[0128] 0.4 parts of crystal nucleating agent, composed of fumed silica, with a particle size of 60 nm;

[0129] The above materials are added into a high-speed mixer and premixed uniformly, and then a twin-screw extruder is used for melting, mixing, extrusion and granulation to obtain a composition; the processing temperatures of each section of the extruder are 185°C, 195°C, 200°C, 210°C, 220°C, 225°C, 210°C, 200°C, 190°C, and the screw speed is 100r / min; the twin-screw extruder used is a large-capacity evaporation (multi-stage exhaust) devolatilization twin-screw unit with a length-to-diameter ratio of 65:1, and the vacuum degree of each exhaust section of the twin-screw extruder during operation is -0.08MPa.

[0130] Example 8

[0131] The polyoxymethylene composition ratio is as follows:

[0132] Copolymer polyoxymethylene resin: 100 parts, melt index 40.0g / 10min;

[0133] 0.6 parts of small molecule formaldehyde absorbent, which is a derivative of melamine, methyl cyanamide, produced by Hubei Fengcheng Chemical Co., Ltd.;

[0134] 0.6 parts of polymer formaldehyde absorbent, which is composed of PA6 / PA1010 copolyamide resin containing hydrazide end groups, in powder form, with a particle size of 25 μm and a melting point of 160°C;

[0135] 0.6 parts of formaldehyde fixative, which is a low molecular weight polyester resin containing hydrazide end groups, with a molecular weight of 2000 g / mol, in powder form, a particle size of 30 μm, and a melting point of 150°C. The manufacturer is Dongrui Chemical Company;

[0136] 0.60 parts of composite antioxidant, the components are triethylene glycol bis-β-(3-tert-butyl-4-hydroxy-5-methylphenyl) propionate / β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate / bis(2,4-di-tert-butylphenol) pentaerythritol diphosphite, the weight ratio of the three components is 1:1:2;

[0137] 0.6 parts of composite formic acid absorbent, composition: Mg6Al2(OH) 16 SO4·4H2O and magnesium stearate compound, the weight ratio of the two is 1:1; Mg6Al2(OH) 16 The particle size of SO4·4H2O is 6 μm;

[0138] 0.3 parts of lubricant, composed of glyceryl monostearate;

[0139] 0.4 parts of crystal nucleating agent, composed of talc powder, with a particle size of 5 μm;

[0140] The above materials are added into a high-speed mixer and premixed uniformly, and then a twin-screw extruder is used for melting, mixing, extrusion and granulation to obtain a composition; the processing temperatures of each section of the extruder are 185°C, 195°C, 200°C, 210°C, 220°C, 225°C, 210°C, 200°C, 190°C, and the screw speed is 100r / min; the twin-screw extruder used is a large-capacity evaporation (multi-stage exhaust) devolatilization twin-screw unit with a length-to-diameter ratio of 65:1, and the vacuum degree of each exhaust section of the twin-screw extruder during operation is -0.08MPa.

[0141] Example 9

[0142] The polyoxymethylene composition ratio is as follows:

[0143] Copolymer polyoxymethylene resin: 100 parts, melt index 2.5g / 10min;

[0144] 0.9 parts of small molecule formaldehyde absorber, which is melamine;

[0145] 0.9 parts of polymer formaldehyde absorbent, composed of PA6 / PA1010 copolyamide resin containing hydrazide end groups, in powder form, with a particle size of 25 μm and a melting point of 160°C;

[0146] 0.8 parts of formaldehyde fixative, composed of low molecular weight polyester resin containing hydrazide end groups, with a molecular weight of 2000 g / mol, in powder form, a particle size of 30 μm, a melting point of 150°C, and produced by Dongrui Chemical Company;

[0147] 0.80 parts of composite antioxidant, the ingredients are triethylene glycol bis-β-(3-tert-butyl-4-hydroxy-5-methylphenyl) propionate / β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate / dioctadecyl pentaerythritol diphosphite, the weight ratio of the three components is 2:1:0.5;

[0148] 0.8 parts of composite formic acid absorbent, composition: Mg6Al2(OH) 16 SO4·4H2O and calcium stearate compound, weight ratio of the two is 1.2:1; Mg6Al2(OH) 16 The particle size of SO4·4H2O is 6 μm;

[0149] 0.5 parts of lubricant, composed of glyceryl monostearate;

[0150] 0.4 parts of crystal nucleating agent, composed of kaolin, with a particle size of 3 μm;

[0151] The above materials are added into a high-speed mixer and premixed uniformly, and then a twin-screw extruder is used for melting, mixing, extrusion and granulation to obtain a composition; the processing temperatures of each section of the extruder are 185°C, 195°C, 200°C, 210°C, 220°C, 225°C, 210°C, 200°C, 190°C, and the screw speed is 100r / min; the twin-screw extruder used is a large-capacity evaporation (multi-stage exhaust) devolatilization twin-screw unit with a length-to-diameter ratio of 65:1, and the vacuum degree of each exhaust section of the twin-screw extruder during operation is -0.08MPa.

[0152] Example 10

[0153] The polyoxymethylene composition ratio is as follows:

[0154] Copolymer polyoxymethylene resin: 100 parts, melt index 2.5g / 10min;

[0155] 0.9 parts of small molecule formaldehyde absorbent, which is a derivative of melamine, methyl cyanamide, produced by Hubei Fengcheng Chemical Co., Ltd.;

[0156] 0.9 parts of polymer formaldehyde absorbent, composed of PA6 / PA1010 copolyamide resin containing hydrazide end groups, in powder form, with a particle size of 25 μm and a melting point of 160°C;

[0157] 0.15 parts of formaldehyde fixative, which is a low molecular weight polyester resin containing hydrazide end groups, with a molecular weight of 2000 g / mol, in powder form, a particle size of 30 μm, and a melting point of 150°C. The manufacturer is Dongrui Chemical Company;

[0158] 0.90 parts of composite antioxidant, the ingredients are triethylene glycol bis-β-(3-tert-butyl-4-hydroxy-5-methylphenyl) propionate / β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate / dioctadecyl pentaerythritol diphosphite, and the weight ratio of the three components is 1:1:1;

[0159] 0.9 parts of composite formic acid absorbent, composition: Mg6Al2(OH) 16 SO4·4H2O and zinc stearate compound, the weight ratio of the two is 1:1; Mg6Al2(OH) 16 The particle size of SO4·4H2O is 6 μm;

[0160] 0.5 parts of lubricant, composed of N,N-ethylene bisstearamide;

[0161] 0.4 parts of crystal nucleating agent, composed of talc powder, with a particle size of 5 μm;

[0162] The above materials are added into a high-speed mixer and premixed uniformly, and then a twin-screw extruder is used for melting, mixing, extrusion and granulation to obtain a composition; the processing temperatures of each section of the extruder are 185°C, 195°C, 200°C, 210°C, 220°C, 225°C, 210°C, 200°C, 190°C, and the screw speed is 100r / min; the twin-screw extruder used is a large-capacity evaporation (multi-stage exhaust) devolatilization twin-screw unit with a length-to-diameter ratio of 65:1, and the vacuum degree of each exhaust section of the twin-screw extruder during operation is -0.08MPa.

[0163] Embodiment 11

[0164] The polyoxymethylene composition ratio is as follows:

[0165] Copolymer polyoxymethylene resin: 100 parts, melt index 9.0g / 10min;

[0166] 0.2 parts of small molecule formaldehyde absorber, which is melamine;

[0167] 0.2 parts of polymer formaldehyde absorbent, composed of PA6 / PA1010 copolyamide resin containing hydrazide end groups, in powder form, with a particle size of 25 μm and a melting point of 160°C;

[0168] 0 parts of formaldehyde fixative, not used;

[0169] 0.20 parts of composite antioxidant, the components are triethylene glycol bis-β-(3-tert-butyl-4-hydroxy-5-methylphenyl) propionate / N, N-bis-(3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionyl) hexanediamine / tris(2,4-di-tert-butylphenyl) phosphite, and the weight ratio of the three components is 1:1:1;

[0170] 0.2 parts of composite formic acid absorbent, composition: Mg6Al2(OH) 16 Compound of CO3·4H2O and zinc stearate, weight ratio of 1:1; Mg6Al2(OH) 16 The particle size of CO3·4H2O is 8 μm;

[0171] 0.1 part of lubricant, composed of N,N-ethylene bisstearamide;

[0172] 0.1 part of crystal nucleating agent, composed of fumed silica, with a particle size of 60 nm;

[0173] The above materials are added into a high-speed mixer and premixed uniformly, and then a twin-screw extruder is used for melting, mixing, extrusion and granulation to obtain a composition; the processing temperatures of each section of the extruder are 185°C, 195°C, 200°C, 210°C, 220°C, 225°C, 210°C, 200°C, 190°C, and the screw speed is 100r / min; the twin-screw extruder used is a large-capacity evaporation (multi-stage exhaust) devolatilization twin-screw unit with a length-to-diameter ratio of 65:1, and the vacuum degree of each exhaust section of the twin-screw extruder during operation is -0.08MPa.

[0174] Example 12

[0175] The polyoxymethylene composition ratio is as follows:

[0176] Copolymer polyoxymethylene resin: 100 parts, melt index 9.0g / 10min;

[0177] 0.2 parts of small molecule formaldehyde absorber, which is melamine;

[0178] 0.2 parts of polymer formaldehyde absorbent, composed of PA6 / PA1010 copolyamide resin containing hydrazide end groups, in powder form, with a particle size of 25 μm and a melting point of 160°C;

[0179] 0.2 parts of formaldehyde fixative, composed of low molecular weight polyester resin containing hydrazide end groups, with a molecular weight of 2000 g / mol, in powder form, a particle size of 30 μm, a melting point of 150°C, and produced by Dongrui Chemical Company;

[0180] 0.20 parts of antioxidant, the ingredient is single triethylene glycol bis-β-(3-tert-butyl-4-hydroxy-5-methylphenyl) propionate;

[0181] 0.2 parts of composite formic acid absorbent, composition: Mg6Al2(OH) 16 Compound of CO3·4H2O and zinc stearate, weight ratio of 1:1; Mg6Al2(OH) 16 The particle size of CO3·4H2O is 8 μm;

[0182] 0.1 part of lubricant, composed of N,N-ethylene bisstearamide;

[0183] 0.1 part of crystal nucleating agent, composed of fumed silica, with a particle size of 60 nm;

[0184] The above materials are added into a high-speed mixer and premixed uniformly, and then a twin-screw extruder is used for melting, mixing, extrusion and granulation to obtain a composition; the processing temperatures of each section of the extruder are 185°C, 195°C, 200°C, 210°C, 220°C, 225°C, 210°C, 200°C, 190°C, and the screw speed is 100r / min; the twin-screw extruder used is a large-capacity evaporation (multi-stage exhaust) devolatilization twin-screw unit with a length-to-diameter ratio of 65:1, and the vacuum degree of each exhaust section of the twin-screw extruder during operation is -0.08MPa.

[0185] Embodiment 13

[0186] The polyoxymethylene composition ratio is as follows:

[0187] Copolymer polyoxymethylene resin: 100 parts, melt index 9.0g / 10min;

[0188] 0.2 parts of small molecule formaldehyde absorber, which is melamine;

[0189] 0.4 parts of adipic acid dihydrazide;

[0190] 0.20 parts of composite antioxidant, the components are triethylene glycol bis-β-(3-tert-butyl-4-hydroxy-5-methylphenyl) propionate / N, N-bis-(3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionyl) hexanediamine / tris(2,4-di-tert-butylphenyl) phosphite, and the weight ratio of the three components is 1:1:1;

[0191] 0.2 parts of composite formic acid absorbent, composition: Mg6Al2(OH) 16 Compound of CO3·4H2O and zinc stearate, weight ratio of 1:1; Mg6Al2(OH) 16 The particle size of CO3·4H2O is 8 μm;

[0192] 0.1 part of lubricant, composed of N,N-ethylene bisstearamide;

[0193] 0.1 part of crystal nucleating agent, composed of fumed silica, with a particle size of 60 nm;

[0194] The above materials are added into a high-speed mixer and premixed uniformly, and then a twin-screw extruder is used for melting, mixing, extrusion and granulation to obtain a composition; the processing temperatures of each section of the extruder are 185°C, 195°C, 200°C, 210°C, 220°C, 225°C, 210°C, 200°C, 190°C, and the screw speed is 100r / min; the twin-screw extruder used is a large-capacity evaporation (multi-stage exhaust) devolatilization twin-screw unit with a length-to-diameter ratio of 65:1, and the vacuum degree of each exhaust section of the twin-screw extruder during operation is -0.08MPa.

[0195] Comparative Example 1

[0196] The polyoxymethylene composition ratio is as follows:

[0197] Copolymer polyoxymethylene resin: 100 parts, melt index 9.0g / 10min;

[0198] 0.2 parts of small molecule formaldehyde absorber, which is melamine;

[0199] 0 parts of polymer formaldehyde absorbent, not used;

[0200] 0.2 parts of formaldehyde fixative, composed of low molecular weight polyester resin containing hydrazide end groups, with a molecular weight of 2000 g / mol, in powder form, a particle size of 30 μm, a melting point of 150°C, and produced by Dongrui Chemical Company;

[0201] 0.20 parts of composite antioxidant, the components are triethylene glycol bis-β-(3-tert-butyl-4-hydroxy-5-methylphenyl) propionate / N, N-bis-(3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionyl) hexanediamine / tris(2,4-di-tert-butylphenyl) phosphite, and the weight ratio of the three components is 1:1:1;

[0202] 0.2 parts of composite formic acid absorbent, composition: Mg6Al2(OH) 16 Compound of CO3·4H2O and zinc stearate, weight ratio of 1:1; Mg6Al2(OH) 16 The particle size of CO3·4H2O is 8 μm;

[0203] 0.1 part of lubricant, composed of N,N-ethylene bisstearamide;

[0204] 0.1 part of crystal nucleating agent, composed of fumed silica, with a particle size of 60 nm;

[0205] The above materials are added into a high-speed mixer and premixed uniformly, and then a twin-screw extruder is used for melting, mixing, extrusion and granulation to obtain a composition; the processing temperatures of each section of the extruder are 185°C, 195°C, 200°C, 210°C, 220°C, 225°C, 210°C, 200°C, 190°C, and the screw speed is 100r / min; the twin-screw extruder used is a large-capacity evaporation (multi-stage exhaust) devolatilization twin-screw unit with a length-to-diameter ratio of 65:1, and the vacuum degree of each exhaust section of the twin-screw extruder during operation is -0.08MPa.

[0206] Comparative Example 2

[0207] The polyoxymethylene composition ratio is as follows:

[0208] Copolymer polyoxymethylene resin: 100 parts, melt index 9.0g / 10min;

[0209] 0.2 parts of small molecule formaldehyde absorber, which is melamine;

[0210] 0.2 parts of polymer formaldehyde absorbent, composed of PA6 / PA1010 copolyamide resin containing hydrazide end groups, in powder form, with a particle size of 25 μm and a melting point of 160°C;

[0211] 0.2 parts of formaldehyde fixative, which is a low molecular weight polyester resin containing hydrazide end groups, with a molecular weight of 2000 g / mol, in powder form, a particle size of 30 μm, and a melting point of 150°C. The manufacturer is Dongrui Chemical Company;

[0212] 0.20 parts of composite antioxidant, the components are triethylene glycol bis-β-(3-tert-butyl-4-hydroxy-5-methylphenyl) propionate / N, N-bis-(3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionyl) hexanediamine / tris(2,4-di-tert-butylphenyl) phosphite, and the weight ratio of the three components is 1:1:1;

[0213] 0 parts of composite formic acid absorbent, not used;

[0214] 0.1 part of lubricant, composed of N,N-ethylene bisstearamide;

[0215] 0.1 part of crystal nucleating agent, composed of fumed silica, with a particle size of 60 nm;

[0216] The above materials are added into a high-speed mixer and premixed uniformly, and then a twin-screw extruder is used for melting, mixing, extrusion and granulation to obtain a composition; the processing temperatures of each section of the extruder are 185°C, 195°C, 200°C, 210°C, 220°C, 225°C, 210°C, 200°C, 190°C, and the screw speed is 100r / min; the twin-screw extruder used is a large-capacity evaporation (multi-stage exhaust) devolatilization twin-screw unit with a length-to-diameter ratio of 65:1, and the vacuum degree of each exhaust section of the twin-screw extruder during operation is -0.08MPa.

[0217] Comparative Example 3

[0218] The polyoxymethylene composition ratio is as follows:

[0219] Copolymer polyoxymethylene resin: 100 parts, melt index 9.0g / 10min;

[0220] 0.2 parts of small molecule formaldehyde absorber, which is melamine;

[0221] 0 parts of polymer formaldehyde absorbent, not used;

[0222] 0 parts of formaldehyde fixative, not used;

[0223] 0.20 parts of composite antioxidant, the components are triethylene glycol bis-β-(3-tert-butyl-4-hydroxy-5-methylphenyl) propionate / N, N-bis-(3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionyl) hexanediamine / tris(2,4-di-tert-butylphenyl) phosphite, and the weight ratio of the three components is 1:1:1;

[0224] 0.2 parts of composite formic acid absorbent, composition: Mg6Al2(OH) 16 Compound of CO3·4H2O and zinc stearate, weight ratio of 1:1; Mg6Al2(OH) 16 The particle size of CO3·4H2O is 8 μm;

[0225] 0.1 part of lubricant, composed of N,N-ethylene bisstearamide;

[0226] 0.1 part of crystal nucleating agent, composed of fumed silica, with a particle size of 60 nm;

[0227] The above materials are added into a high-speed mixer and premixed uniformly, and then a twin-screw extruder is used for melting, mixing, extrusion and granulation to obtain a composition; the processing temperatures of each section of the extruder are 185°C, 195°C, 200°C, 210°C, 220°C, 225°C, 210°C, 200°C, 190°C, and the screw speed is 100r / min; the twin-screw extruder used is a large-capacity evaporation (multi-stage exhaust) devolatilization twin-screw unit with a length-to-diameter ratio of 65:1, and the vacuum degree of each exhaust section of the twin-screw extruder during operation is -0.08MPa.

[0228] Comparative Example 4

[0229] The polyoxymethylene composition ratio is as follows:

[0230] Copolymer polyoxymethylene resin: 100 parts, melt index 9.0g / 10min;

[0231] 0.2 parts of small molecule formaldehyde absorber, which is melamine;

[0232] 0 parts of polymer formaldehyde absorbent, not used;

[0233] 0 parts of formaldehyde fixative, not used;

[0234] 0.20 parts of composite antioxidant, the components are triethylene glycol bis-β-(3-tert-butyl-4-hydroxy-5-methylphenyl) propionate / N, N-bis-(3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionyl) hexanediamine / tris(2,4-di-tert-butylphenyl) phosphite, and the weight ratio of the three components is 1:1:1;

[0235] 0 parts of composite formic acid absorbent, not used;

[0236] 0.1 part of lubricant, composed of N,N-ethylene bisstearamide;

[0237] 0.1 part of crystal nucleating agent, composed of fumed silica, with a particle size of 60 nm;

[0238] The above materials are added into a high-speed mixer and premixed uniformly, and then a twin-screw extruder is used for melting, mixing, extrusion and granulation to obtain a composition; the processing temperatures of each section of the extruder are 185°C, 195°C, 200°C, 210°C, 220°C, 225°C, 210°C, 200°C, 190°C, and the screw speed is 100r / min; the twin-screw extruder used is a large-capacity evaporation (multi-stage exhaust) devolatilization twin-screw unit with a length-to-diameter ratio of 65:1, and the vacuum degree of each exhaust section of the twin-screw extruder during operation is -0.08MPa.

[0239] Comparative Example 5

[0240] The common commercially available MC90 copolymer formaldehyde is produced by the National Energy Ningmei Group and has a melting point of 9.3g / 10min.

[0241] The polyoxymethylene prepared in the above examples and comparative examples was subjected to performance tests, and the test method is as follows.

[0242] The method for determining the formaldehyde emission of the polyoxymethylene composition is as follows:

[0243] A 200g polyoxymethylene sample was purged in a sealed container using a high-purity nitrogen stream, and the purge gas was bubbled through a washing bottle filled with 1500mL of deionized water. During the experiment, the polyoxymethylene sample temperature was 150°C and the test time was 60min. After the test, the formaldehyde concentration in the deionized water of the washing bottle was accurately measured using the well-known acetylacetone ultraviolet spectrophotometry method, and then converted into formaldehyde release. The principle of the acetylacetone method is to use formaldehyde, acetylacetone and ammonia to generate a yellow compound 3,5-diacetyl 1,4-dihydrolutidine, and perform spectrophotometric determination at a wavelength of 412nm.

[0244] The determination methods of other properties of the polyoxymethylene composition are as follows:

[0245] Melt index is based on ISO 1133, 190°C, 2.16kg;

[0246] Tensile strength according to standard ISO527-1,2;

[0247] Bending strength is based on standard ISO178;

[0248] Charpy notched impact strength is based on ISO 179-1 2001.

[0249] The test results of the polyoxymethylene samples obtained in the examples and comparative examples are shown in Table 1.

[0250] Table 1

[0251] Formaldehyde emission (ppm) Melt index (g / 10min) Tensile strength(MPa) Bending strength(MPa) <![CDATA[Notched impact strength of simply supported beam (kJ / m 2 )]]> Example 1 7.2 8.8 61.3 82.9 6.5 Example 2 8.0 9.1 60.9 81.8 6.4 Example 3 4.9 8.7 62.2 83.4 6.7 Example 4 3.8 27.1 62.8 90.7 3.9 Example 5 2.3 28.7 61.6 92.6 4.2 Example 6 8.0 27.2 63.7 89.7 4.5 Example 7 7.6 26.5 59.8 88.2 3.8 Example 8 6.9 40.2 64.5 91.1 3.0 Example 9 3.7 2.5 58.7 80.8 8.7 Example 10 6.1 2.5 59.3 79.8 8.8 Embodiment 11 12.7 9.0 61.8 82.5 6.5 Example 12 13.5 9.1 62.0 81.9 6.5 Embodiment 13 16.4 9.6 61.7 80.6 6.4 Comparative Example 1 12.6 8.8 61.0 82.0 6.7 Comparative Example 2 26.7 8.7 60.3 83.1 6.4 Comparative Example 3 72.5 8.8 60.9 82.3 6.3 Comparative Example 4 105.2 9.4 59.3 80.9 6.0 Comparative Example 5 135.2 9.3 61.3 81.5 6.4

[0252] From the above description, it can be seen that the above embodiments of the present invention achieve the following technical effects: the formaldehyde absorbent, the composite antioxidant, and the formic acid absorbent can produce a significant synergistic effect, which can greatly reduce the formaldehyde release in the polyoxymethylene composition. The extremely low small molecule substance release polyoxymethylene composition provided by the present invention is significantly superior to other polyoxymethylene compositions in formaldehyde release, and is easy to be industrially applied.

[0253] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A polyoxymethylene composition, characterized in that: include: In parts by weight, 100 parts of polyoxymethylene resin, 0.04-2 parts of formaldehyde absorbent, 0.20-1 parts of antioxidant, 0.02-1 parts of formic acid absorbent, 0.05-1 parts of lubricant and 0.02-0.5 parts of crystal nucleating agent, wherein the formaldehyde absorbent includes a small molecular formaldehyde absorbent and a high molecular formaldehyde absorbent; The small molecule formaldehyde absorbent includes any one or more of melamine and melamine derivatives; The polymer formaldehyde absorbent is a copolyamide resin containing hydrazide end groups, the content of the polymer formaldehyde absorbent is 0.02-1 parts by weight, the particle size of the polymer formaldehyde absorbent is ≤55 μm, and the melting point of the polymer formaldehyde absorbent is greater than 140° C. The antioxidant is a composite antioxidant, which includes a first antioxidant, a second antioxidant and a third antioxidant, wherein the first antioxidant includes triethylene glycol bis-β-(3-tert-butyl-4-hydroxy-5-methylphenyl) propionate, the second antioxidant includes N,N-bis-(3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionyl) hexanediamine, tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate] pentaerythritol ester and β-(3, The third antioxidant comprises any one or more of tris(2,4-di-tert-butylphenyl) phosphite, dioctadecyl pentaerythritol diphosphite and bis(2,4-di-tert-butylphenol) pentaerythritol diphosphite, and the weight ratio of the first antioxidant, the second antioxidant and the third antioxidant is 1: (0.25-1.5): (0.25-2.5); The formic acid absorbent is a compound of an inorganic compound represented by Formula I and stearate. Mg 1-x Al x (OH)2 A n- x / n ·mH2O formula I In the formula, A n- It is an n-valent anion, n is an integer of 1-3, x=0.2-0.33, and m is 2-6; The composition also includes 0.01-2 parts by weight of a formaldehyde fixative, which is a low molecular weight polyester resin containing hydrazide end groups, has a molecular weight of 1000-5000 g / mol, a particle size of 55 μm or less, and a melting point of greater than 130° C.

2. The polyoxymethylene composition according to claim 1, characterized in that The particle size of the inorganic compound is less than or equal to 10 μm.

3. The polyoxymethylene composition according to claim 1, characterized in that The stearate is selected from any one or more of calcium stearate, barium stearate, zinc stearate and magnesium stearate.

4. The polyoxymethylene composition according to claim 1, characterized in that The weight ratio of the inorganic compound to the stearate is 4:6 to 6:

4.

5. The polyoxymethylene composition according to claim 1, characterized in that: The melt index of the polyoxymethylene resin is 1.0-550.0 g / 10 min; And / or, the lubricant includes any one or more of N,N-ethylene bisstearamide and glyceryl monostearate.

6. The polyoxymethylene composition according to claim 1, characterized in that The crystal nucleating agent is any one or more of fumed silica, talc and kaolin.

7. The polyoxymethylene composition according to claim 6, characterized in that: The particle size of the fumed silica is not greater than 100 nm; The particle size of the talc powder is not greater than 8 μm; the particle size of the kaolin is not greater than 8 μm.

8. A method for preparing a polyoxymethylene material, characterized in that: include: The polyoxymethylene composition according to any one of claims 1 to 7 is added into a stirrer for uniform premixing, and then melted, mixed and granulated by a twin-screw extruder to obtain a polyoxymethylene material.

9. The preparation method according to claim 8, characterized in that: The temperature of each section of the extruder is 170-245° C., and the rotation speed of the twin-screw extruder is 20-600 r / min.

10. The preparation method according to claim 9, characterized in that: The aspect ratio of the twin-screw extruder is 25-70:1, and the vacuum degree of each exhaust section of the twin-screw extruder is ≤-0.06MPa during operation.

11. A polyoxymethylene material, characterized in that: The polyoxymethylene composition is prepared from any one of claims 1 to 7, or is prepared by the preparation method according to any one of claims 8 to 10.

Citation Information

Patent Citations

  • Low VOC (volatile organic compound) polyformaldehyde (POM) material and preparation method thereof

    CN104004317A

  • Preparation method of low-VOC (volatile organic chemical) polyformaldehyde composite plastic for automobile trims

    CN108440896A

  • Low-release polyformaldehyde and preparation method thereof

    CN113831681A

  • Formaldehyde-removal composition, humidifying composite compound and humidifying container

    CN101011592A

  • Low formaldehyde emission polyacetal composition

    CN101993579A