Metal materials for plastic processing

By forming a double-layer film structure on the surface of metal materials for plastic processing, and using a second film with a compound directly bonded to the benzene ring or its salt or peroxide, the problem of welding during plastic processing is solved and the melt resistance is significantly improved. Weldability and extended mold life.

CN116200733BActive Publication Date: 2024-10-25NIHON PARKERIZING CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310185445.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2018-02-28
Filing Date
2019-02-22
Publication Date
2024-10-25
Estimated Expiration
2039-02-22

AI Technical Summary

Technical Problem

Existing metal materials used for plastic processing are prone to welding during forging and other processes, resulting in changes in mold size and shortened use times, which increase costs.

Method used

A double-layer film structure is formed on the surface of the metal material, in which the first film is composed of chemical synthesis or coating materials, and the second film contains a compound directly bonded to a benzene ring or its salt or peroxide to improve welding resistance. .

Benefits of technology

It effectively prevents welding during plastic processing, extends the service life of the mold, and reduces production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116200733B_ABST
    Figure CN116200733B_ABST
Patent Text Reader

Abstract

The technical problem of the present invention is to provide a metal material for plastic working with excellent resistance to fusion welding. The above technical problem can be solved by the metal material for plastic working of the present invention, which has a first film on the surface of the metal material, a second film on the surface of the first film or on the surface, the second film is a surface layer, and the second film contains a compound having a benzene ring directly bonded to at least one carboxyl group, or a salt thereof, or a peroxide thereof.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application is a divisional application of the invention patent application with application number 201980014024.3. The application date of the original application is February 22, 2019, and the name of the invention is “Metal Materials for Plastic Working”. Technical Field

[0002] The present invention relates to a metal material for plastic working, which has a film required when plastic working such as forging (including cold, warm and hot forging), wire drawing and tube drawing is performed on a steel material or other metal material. Background Art

[0003] In the plastic processing of metal materials, the mold and the metal material for plastic processing may sometimes be welded. Fusion welding not only fails to obtain the intended molded object, but also causes the size of the mold to change due to the influence of the welded metal, shortening the number of times the mold can be used. Therefore, the mold has to be remade, which reduces cost-effectiveness. Therefore, a metal material for plastic processing with excellent resistance to fusion welding is required.

[0004] For example, Patent Document 1 discloses a lubricant for warm plastic working and hot plastic working, which contains an alkali metal salt of an aromatic carboxylic acid compound having two or more carboxyl groups, several types of water-soluble polymer compounds, and water.

[0005] Patent Document 2 discloses a lubricant for warm forging and hot forging, which contains a specific compound in which two aromatic rings are bonded, and the aromatic rings have two carboxyl groups located at ortho positions.

[0006] Patent Document 3 discloses an aqueous cold plastic working lubricant composition comprising an aromatic carboxylate having a melting point of 90° C. or higher formed of sodium hydroxide or potassium hydroxide, a water-soluble polymer compound and / or wax, and water.

[0007] Prior art literature

[0008] Patent Literature

[0009] Patent Document 1: Japanese Patent Application Publication No. 2015-89938;

[0010] Patent Document 2: Japanese Patent Application Publication No. 2015-89939;

[0011] Patent document 3: Japanese Patent Application Publication No. 2015-17171. Summary of the invention

[0012] Problem that the invention aims to solve

[0013] An object of the present invention is to provide a metal material for plastic working having excellent resistance to fusion welding.

[0014] Solutions for solving problems

[0015] The present inventors have conducted intensive research to solve the above-mentioned problems, and as a result, have discovered a metal material for plastic working with excellent resistance to welding, which has a first film on the surface or on the surface of the metal material, and a second film on the surface or on the surface of the above-mentioned first film, wherein the above-mentioned second film is a surface layer, and the above-mentioned second film contains a compound having a benzene ring directly bonded to at least one carboxyl group, or a salt thereof, or a peroxide thereof, thereby completing the present invention.

[0016] The present invention (1) is a metal material for plastic working,

[0017] It has a first film on the surface of the metal material or on the surface thereof,

[0018] A second film is provided on the surface of the first film or on the surface thereof,

[0019] The second membrane is the surface layer.

[0020] The second film includes a compound having a benzene ring directly bonded to at least one carboxyl group, a salt thereof, or a peroxide thereof.

[0021] Effects of the Invention

[0022] According to the present invention, it is possible to provide a metal material for plastic working which is excellent in the effect of preventing welding caused by friction between a die and the metal material for forming (welding resistance) occurring during plastic working. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 This is a diagram showing the evaluation criteria for the welding resistance of the test pieces subjected to the processability evaluation test (using photographs as drawings). DETAILED DESCRIPTION

[0024] Hereinafter, the contents of the present invention will be described in detail.

[0025] <Metal materials for plastic working>

[0026] A metal material for plastic working as one embodiment of the present invention comprises: a metal material, a first film on the surface of the metal material or on the surface, and a second film on the surface of the first film or on the surface, wherein the second film comprises a compound having a benzene ring directly bonded to at least one carboxyl group or a salt thereof, or a peroxide thereof. In addition, between the first film and the second film, there may be a single-layer or multi-layered film, as long as the second film is present in the surface layer.

[0027] The plastic working in this specification is not particularly limited as long as it is a known plastic working, and examples thereof include forging (cold, warm, hot), extrusion, wire drawing, tube drawing, drawing, rolling, bending, joining, shearing, shaping, etc. Among them, the metal material for plastic working of the present invention is preferably used for plastic working in which a particularly large load is applied to the metal material, such as forging, wire drawing, and tube drawing.

[0028] 1. Composition of metal materials for plastic processing

[0029] 1-1. Metal materials

[0030] The metal material is not particularly limited, and is generally a metal material used for plastic working, and examples thereof include iron, iron alloys (steel, stainless steel, etc.), aluminum, aluminum alloys, magnesium, magnesium alloys, titanium, titanium alloys, copper, copper alloys, tin, tin alloys, zinc, zinc alloys, and the like.

[0031] As long as the effect of the present invention is not impaired, the metal material may also be a plated material having a plated film. The material of the plated film is not particularly limited, and for example, metals such as nickel, iron, aluminum, manganese, chromium, magnesium, cobalt, lead, zinc, tin or antimony or alloys of various metals may be used, and further, metals containing inevitable impurities or alloys of various metals may be used.

[0032] When the plated film is artificially formed, a known method can be used for the formation method, and examples thereof include electroplating (electrolytic plating, electroplating), electroless plating, hot dip plating, vapor phase plating, mechanical plating, thermal spraying, and the like.

[0033] The thickness of the plated film is not particularly limited, and is, for example, 0.1 μm or more and 1000 μm or less.

[0034] In addition, an oxide film may be formed on the surface of the metal material. The oxide film is not particularly limited and may be a natural oxide film naturally generated in the atmosphere or an artificially formed oxide film.

[0035] There are no particular limitations on the method for forming an artificial oxide film, and examples thereof include: an anodic oxidation method by passing electricity through an electrolyte solution using a metal material as an anode, a method of immersing in a strong acidic liquid, a method of electrolytic polishing, and a method of plasma electrolysis, etc. In addition, the oxide film may be sealed by a steam method, a pure water boiling water method, a nickel acetate method, a dichromic acid method, a sodium silicate method, etc.

[0036] The thickness of the oxide film is not particularly limited, and is, for example, 0.001 μm or more and 100 μm or less.

[0037] The shape of the metal material is not limited to a blank form such as a rod-shaped material or a block-shaped material, and may be a processed shaped part (gear, shaft, etc.), and is not particularly limited.

[0038] 1-2. 1st membrane

[0039] The first film is not particularly limited, and for example, a chemically synthesized film or a coating film can be used.

[0040] 1-2-1. Chemically synthesized membrane

[0041] An example of the film deposition mechanism of chemical conversion treatment is as follows. When a metal material is brought into contact with a chemical conversion treatment agent, the surface of the metal material is etched by H, which is an acid component (etching component) in the chemical conversion treatment agent. + Ion etching (dissolution) causes the pH near the surface to rise. As the pH near the surface rises, the etched metal components in the metal material near the surface and the components contained in the chemical synthesis treatment solution are precipitated on the surface of the metal material in the form of insoluble salts. The insoluble salt forms a film.

[0042] The chemically synthesized film is not particularly limited and is composed of, for example, phosphates, oxalates, aluminates, chromates, molybdates, zirconium compounds, titanium compounds, vanadium compounds, and hafnium compounds. In addition, they may be composed of a single salt or a plurality of salts. The chemically synthesized film is preferably composed of phosphates, oxalates, and aluminates, and more preferably composed of zinc phosphate and iron oxalate.

[0043] The phosphate is not particularly limited, and examples thereof include zinc phosphate, zinc iron phosphate, nickel phosphate, manganese phosphate, iron manganese phosphate, calcium phosphate, cobalt phosphate, magnesium phosphate, aluminum phosphate, sodium phosphate, potassium phosphate, ammonium phosphate, etc. When the metal material is steel, stainless steel, etc., the phosphate is preferred.

[0044] The oxalate is not particularly limited, and examples thereof include sodium oxalate, potassium oxalate, iron oxalate, and ammonium oxalate. When the metal material is stainless steel or the like, the oxalate is preferred.

[0045] The aluminate is not particularly limited, and examples thereof include lithium aluminate, sodium aluminate, potassium aluminate, magnesium aluminate, calcium aluminate, etc. When the metal material is aluminum or an aluminum alloy, the aluminate is preferred.

[0046] The amount of the chemically synthesized film applied is not particularly limited, but is, for example, 0.5 g / m 2 Above and 20.0g / m 2 Below, preferably 2.0g / m 2 Above and 10.0g / m 2The above-mentioned adhesion amount can be adjusted by changing the composition, concentration, etc. of the chemical conversion treatment agent, or by changing the contact conditions such as the contact method, contact temperature, and contact time.

[0047] 1-2-2. Coating

[0048] The coating film is formed by applying a coating agent on the surface of a metal material.

[0049] The material of the coating film is not particularly limited as long as it can be formed on the surface of the metal material of the present embodiment and can form the second film on the surface of the metal material. Examples of coatings formed using a coating-type coating agent include: coatings formed by a coating-type chromate treatment using a treatment solution containing chromic acid, dichromic acid or a salt thereof as a main component; coatings formed by a coating-type chromate-free treatment without adding chromic acid or dichromic acid; coatings formed from a silane coupling agent monomer; coatings of silica, silica colloid, etc. modified with a silane coupling agent or the like; organic resin coatings containing polyurethane resins, epoxy resins, acrylic resins, olefin resins such as polyethylene, polypropylene, and ethylene-acrylic acid copolymers, styrene resins such as polystyrene, polyesters, or copolymers or modified products thereof; inorganic coatings containing glass such as lithium silicate and sodium silicate, metal oxyacid salts, metal hydroxides, metal phosphates, metal fluoride compounds, etc. (except for plated coatings and oxide coatings); coatings in which a lubricant is dispersed in a solvent such as water or oil or in a base polymer such as a copolymer of styrene and maleic acid / maleic anhydride, etc.

[0050] The solid lubricant is not particularly limited, and examples thereof include waxes such as polyethylene wax and polypropylene wax; layered clay minerals such as montmorillonite, vermiculite, mica, brittle mica, pyrophyllite and kaolinite; polytetrafluoroethylene; fatty acid metal soaps, fatty acid amides; molybdenum disulfide; tungsten disulfide; graphite; and melamine cyanurate.

[0051] 1-3. Second membrane

[0052] 1-3-1. Material

[0053] The second film of the present embodiment comprises at least one of the following: a compound having a benzene ring directly bonded to at least one carboxyl group in its structure, or a salt thereof, or a peroxide thereof. In this specification, a compound having a benzene ring directly bonded to at least one carboxyl group is sometimes described as an aromatic carboxylic acid compound.

[0054] Here, the benzene ring in the present invention refers to a compound having a single benzene ring such as a benzene compound, but is not limited thereto and also includes condensed polycyclic aromatic hydrocarbons such as naphthalene and anthracene in which a plurality of benzene rings are directly condensed.

[0055] The aromatic carboxylic acid compound is not particularly limited as long as the effect of the present invention is not impaired, and examples thereof include pyromellitic acid, xylene acid, mellitic acid, mesitylene acid, prehnitylic acid, durylic acid, β-isoduronic acid, α-isoduronic acid, anisic acid, o-cresotic acid, m-methylsalicylic acid, p-methylsalicylic acid, o-pyrocatechuic acid, β-resorcylic acid, gentisic acid, γ-resorcylic acid, protocatechuic acid, α-resorcylic acid, vanillic acid, isovanillic acid, veratric acid, 2,3-dimethoxybenzoic acid, glycosyl acid, m-hemipic acid, gallic acid, syringic acid, asaronic acid, homophthalic acid acid), homoisophthalic acid, homoterephthalic acid, phthalic acid, isophthalic acid, terephthalic acid, cumic acid, uvitic acid, benzoic acid, phthalic acid, salicylic acid, etc. These may be contained alone or in combination.

[0056] Among the salts of aromatic carboxylic acid compounds, ammonium salts, sodium salts, lithium salts and potassium salts of the above aromatic carboxylic acid compounds are more preferred because they are excellent in the effect of preventing welding during plastic working (welding resistance).

[0057] In addition, for the salt of the aromatic carboxylic acid compound, when multiple carboxyl groups are directly bonded to the benzene ring, at least a portion of them may be salted, or all of them may be salted. For example, in the case of a sodium salt of phthalic acid having two carboxyl groups, it may include sodium hydrogen phthalate in which a single carboxyl group is salted with sodium, and disodium phthalate in which a double carboxyl group is salted with sodium.

[0058] The peroxide of an aromatic carboxylic acid compound is a compound having a peroxide structure at least one of the carboxyl groups directly bonded to the benzene ring of the aromatic carboxylic acid compound. For example, when the aromatic carboxylic acid compound is benzoic acid, its peroxide is benzoic acid peroxide.

[0059] When a plurality of carboxyl groups of the peroxide of the aromatic carboxylic acid compound are directly bonded to the benzene ring, at least a part of the peroxide may have a peroxide structure.

[0060] The aromatic carboxylic acid compound or its salt, or its peroxide, does not necessarily need to be contained in the raw material, as long as it is contained in the formed second film. For example, the anhydride of a carboxylic acid directly bonded to a benzene ring (e.g., phthalic anhydride) is reacted with water or an alcohol to generate a compound having a benzene ring bonded to a carboxyl group.

[0061] The content of the aromatic carboxylic acid compound in the second film is not particularly limited. The second film may contain compounds other than the aromatic carboxylic acid compound, such as other resins, within the range that does not impair the effect of the present invention. In the case where the second film contains compounds other than the aromatic carboxylic acid compound, the content of the aromatic carboxylic acid compound in the second film may be 0.5% by weight or more, preferably 10% by weight or more. The second film may be formed only of the aromatic carboxylic acid compound.

[0062] 1-4. Membrane included between the first membrane and the second membrane

[0063] The metal material for plastic working may include a single layer or a plurality of layers stacked between the first film and the second film.

[0064] The film included between the first film and the second film, the type of film, the material, the combination of materials, the combination of film treatment methods, the number of layers, the thickness of each film, etc. are not particularly limited as long as the effects of the present invention are not impaired.

[0065] The film included between the first film and the second film may include a chemically synthesized film, a coating film, a plated film, an oxidized film, etc. For example, a plated film may be formed on the first film by vapor deposition, and then a chemically synthesized film may be formed on the plated film.

[0066] 2. Method for manufacturing metal material for plastic processing

[0067] Another embodiment of the present invention provides a method for manufacturing a metal material for plastic working, comprising: a first film forming step of forming a first film at least on the surface or surface of the metal material; and a second film forming step of forming a second film on the surface or surface of the first film.

[0068] A water washing step may be included before or after each step in the first film forming step, and a drying step may be included after the first film is formed. In addition, in the second film forming step, a water washing step may be included before or after each step, and a drying step may be included after the second film is formed. Furthermore, when a surface treatment layer is formed between the first film and the second film, a water washing step may be included between the steps, and a drying step may be included after the film is formed.

[0069] Furthermore, if necessary, after forming the first film and before forming the second film, a step of forming a single-layer or multi-layered film may be included.

[0070] Furthermore, a cleaning step may be included before and after each step. In addition, the cleaning step may be performed multiple times.

[0071] 2-1. First film forming step

[0072] The first film forming step may include at least one of a chemical synthesis film forming step and a coating film forming step.

[0073] 2-1-1. Chemical synthesis film formation process

[0074] The chemical synthesis film forming step includes at least a contact step: a chemical synthesis treatment agent is brought into contact with the surface of the metal material to form a first film as a chemical synthesis film. As a contact method, a known method can be used without particular limitation. For example, an electrolytic treatment method performed by passing an electric current, and a treatment method performed without passing an electric current such as an immersion treatment method, a spray treatment method, and a sprinkling treatment method can be cited.

[0075] The (contact) temperature of the metal material and the chemical conversion treatment agent is not particularly limited, but is, for example, preferably 10° C. or higher and 98° C. or lower, and more preferably 20° C. or higher and 50° C. or lower.

[0076] The contact time is not particularly limited, but is preferably, for example, 30 to 300 seconds, and more preferably 60 to 180 seconds.

[0077] 2-1-2. Coating film forming process

[0078] The coating film forming process at least includes the following steps: contacting the treatment agent for forming the film with the surface or the surface of the metal material to form the first film as the coating film. As a contact method, a known method can be used, which is not particularly limited. The coating film can be formed by implementing, for example, a roller pressing method, an immersion method, a flow coating method, a spray method, a brush coating method, an electrostatic coating method, a rod coating method, a powder coating method, etc. More specifically, when, for example, the metal material is in a sheet shape, a roller coating method and a spray coating method are preferably implemented. In addition, if the metal material is a molded product, an immersion method is preferably implemented. In addition, when the raw material contains a solid, the solid raw material can be pre-dissolved or dispersed in a solvent such as water or an organic solvent, and then the treatment agent is prepared.

[0079] The adhesion amount of the coating film is not particularly limited, and is, for example, 0.5 g / m 2 Above and 50.0g / m 2 Below, preferably 2.0g / m 2 Above and 20.0g / m 2 Below, more preferably 2.0g / m2 Above and 10.0g / m 2 The above-mentioned adhesion amount can be adjusted by changing the composition, concentration, etc. of the treatment agent, or by changing the contact conditions such as the contact method, contact temperature, and contact time.

[0080] The contact conditions of the above-mentioned treatment agent are not particularly limited. For example, the temperature of the treatment agent when contacting the above-mentioned treatment agent is 10° C. or higher and 80° C. or lower, preferably 25° C. or higher and 75° C. or lower, more preferably 25° C. or higher and 60° C. or lower, but it is not limited to these temperatures. In addition, the contact time can be appropriately set, and is usually 2 seconds or higher and 180 seconds or lower.

[0081] The first film forming step can include a drying step as required. The drying method can use a known method, and is not particularly limited. For example, natural drying, reduced pressure drying, convection heating drying (such as natural convection heating drying, forced convection heating drying), radiation drying (such as near-infrared drying, far-infrared drying), ultraviolet curing drying, electron beam curing drying, vapor curing (vapor cure), etc. can be mentioned. In addition, a plurality of them can also be used in combination.

[0082] The drying time can be appropriately selected under the most suitable conditions according to the composition of the treatment agent. The drying time is preferably in the range of 1 second to 1800 seconds, and more preferably in the range of 10 seconds to 1200 seconds.

[0083] The drying temperature can be any normal drying temperature, and the metal peak temperature (PMT) of the metal material is preferably above 60°C and below 150°C, and more preferably above 80°C and below 150°C. When the drying temperature is less than 60°C, sometimes, water as the main solvent of the surface treatment agent will remain, resulting in the film being unable to be fixed on the surface of the metal material. In this case, the temperature can also be maintained at a temperature less than 60°C until the water evaporates. Since continuous drying until the water evaporates will reduce productivity, the above-mentioned drying temperature of 60°C or above is preferred.

[0084] 2-2. Method for forming a film included between the first film and the second film

[0085] The method for manufacturing the film included between the first film and the second film includes a film forming step: forming a desired single-layer or multi-layer laminated film on the surface of the first film. The above-mentioned film forming step is not particularly limited, and a known method corresponding to the film to be formed can be used. For example, a chemical synthesis treatment step for forming a chemical synthesis film, a contact step and a drying step of a treatment agent for forming a coating and a metal material forming the first film, a plating treatment step for forming a plated film, etc. The processing conditions of each step are not particularly limited, and processing conditions suitable for each film and its formation method can be used.

[0086] 2-3. Second film forming step

[0087] The second film forming step includes the following steps: contacting the treatment agent for forming the second film with the surface or surface of the first film formed on the surface of the metal material. As a contact method, a known method can be used, and there is no particular limitation. The same method as the contact method in the above-mentioned film forming step can be used. In addition, when the raw material includes a solid, the solid raw material can be pre-dissolved or dispersed in a solvent such as water or an organic solvent, and then the treatment agent is prepared.

[0088] The contact conditions of the treatment agent are not particularly limited. For example, the temperature of the treatment agent when contacting the treatment agent is 10° C. or higher and 80° C. or lower, preferably 25° C. or higher and 75° C. or lower, and more preferably 25° C. or higher and 60° C. or lower, but not limited to these temperatures. In addition, the contact time can be appropriately set, but is usually 2 seconds or higher and 180 seconds or lower.

[0089] The second film forming step may include a drying step as needed. The drying method is not limited to the contact method of the coating film, and the same method as the drying method of the coating film may be used.

[0090] The drying time can be optimally selected according to the composition of the treatment agent, but is preferably within a range of 1 second to 1800 seconds, more preferably 10 seconds to 1200 seconds, from the viewpoint of productivity and film formation.

[0091] The drying temperature may be any normal drying temperature, and the metal peak temperature (PMT) of the metal material is preferably 60° C. or higher and 150° C. or lower, and more preferably 80° C. or higher and 150° C. or lower. When the drying temperature is 60° C. or higher, water as the main solvent of the surface treatment agent is unlikely to remain, and the film is easily fixed on the surface of the metal material, which is also preferred for corrosion resistance.

[0092] The amount of the second film applied is not particularly limited, but is, for example, 0.1 g / m 2 Above and 20.0g / m2 Below, preferably 2.0g / m 2 Above and 15.0g / m 2 The above-mentioned adhesion amount can be adjusted by changing the composition, concentration, etc. of the treatment agent, or by changing the contact conditions such as the contact method, contact temperature, and contact time.

[0093] 2-4. Cleaning process

[0094] The cleaning step is a step of cleaning the surfaces of the metal material, the first film, and each film included between the first film and the second film by, for example, water washing (eg, hot water washing), solvent washing, alkaline degreasing washing, acid washing, or the like.

[0095] The cleaning process is implemented for the purpose of removing oil, dirt and scale attached to the surface or surfaces of the metal material, the first film and each film included between the first film and the second film during the operation. In addition, rust-proof oil is sometimes applied to the surface or surfaces of the metal material for rust prevention. In this case, the purpose also includes removing the rust-proof oil. By implementing the cleaning process, the above-mentioned surface or surfaces can be cleaned, and the treatment agent of the film stacked on the surface or surfaces can be made to contact the above-mentioned surface evenly. In addition, when there is no oil or dirt on the above-mentioned surface or surfaces, and the above-mentioned chemical synthesis treatment agent and coating can be made to contact evenly, there is no need to perform this cleaning process in particular.

[0096] 3. Plastic processing method

[0097] The plastic working method of the present embodiment is not particularly limited, and examples thereof include known methods such as forging, extrusion, wire drawing, tube drawing, drawing, rolling, bending, joining, shearing, and shaping.

[0098] Example

[0099] Hereinafter, the effects of the present invention will be specifically described by giving examples of the present invention and comparative examples. However, the present invention is not limited to these examples.

[0100] (1-1) The shape of the metal material used in Metal Material Examples 1 to 19 and Comparative Examples 1 to 4 is based on the barrel-shaped shape with an upsetting ratio of 45% used in the ball reduction extrusion friction test method disclosed in the reference (Akira Takahashi, Hirose Hitoshi, Shinobu Komiya, Zhigang Wang: Proceedings of the 62nd Annual Conference on Plastic Processing, (2011), 89-90).

[0101] As for the material of the metal material, S10C material was used in Examples 1 to 10 and Comparative Examples 1, 3, and 4, and SUS430 material was used in Examples 11 to 19 and Comparative Example 2.

[0102] (1-2) Preparation of various surface treatment agents

[0103] The surface treatment agents for forming the first and second films of Examples 1 to 19 were prepared in the combinations shown in Table 1. Hereinafter, the surface treatment agent for forming the first film is referred to as surface treatment agent A, and the surface treatment agent for forming the second film is referred to as surface treatment agent B.

[0104] Surface treatment agent A

[0105] The surface treatment agent A of Examples 1 to 10 was prepared. First, Palbond 181XM (manufactured by Nippon Parkersei Co., Ltd.) was added to deionized water in a concentration of 90.0 g / L. Then, the total acidity value obtained by titration was divided by the free acidity value obtained by the same method to obtain the acid ratio (total acidity / free acidity), and the acid ratio was confirmed to be 6.5.

[0106] Next, the accelerator concentration (unit: dots) was adjusted to 2.5 dots using accelerator 131 (manufactured by Nippon Parkersei Co., Ltd.).

[0107] The concentration of the accelerator 131 is measured using a glass instrument called a saccharimeter (capacity 50 mL). In the concentration measurement, the surface treatment agent to which the accelerator is added is filled into the saccharimeter, and 5 g of the reagent 205 (manufactured by Japan Parkersei Co., Ltd.) that reacts with the accelerator contained in the surface treatment agent is added. At this time, if the surface treatment agent contains an accelerator, gas will be generated. The volume of the generated gas represents the concentration of the accelerator, and if the amount of the generated gas is 1 mL, the concentration of the accelerator contained in the surface treatment agent (unit: point) is 1 point.

[0108] Surface treatment agent A of Examples 11 to 19 was prepared. First, Felbond A1 and Felbond A2 (both manufactured by Nippon Parkersei Co., Ltd.) were added to deionized water at a concentration of 40.0 g / L for the former and 20.0 g / L for the latter. Next, the concentration of the accelerator was adjusted to 1.0 using accelerator 16 (manufactured by Nippon Parkersei Co., Ltd.).

[0109] The concentration of the accelerator 16 is titrated as follows: the surface treatment liquid is collected in a beaker using a 25 mL full pipette, 50 mL of deionized water, 25.0 mL of reagent 54 (manufactured by Nippon Parker Seiki Co., Ltd.), and indicator 10 (manufactured by Nippon Parker Seiki Co., Ltd.) are added, and titration is performed with titration solution 53 (manufactured by Nippon Parker Seiki Co., Ltd.) until the liquid turns dark blue. The amount of the titration solution 53 added until then is taken as the accelerator concentration (unit: point).

[0110] Surface treatment agent B

[0111] The surface treatment agent B was prepared by adding the aromatic carboxylic acid compound, its salt, or its peroxide listed in Table 1 to distilled water. The concentration of the aromatic carboxylic acid compound, its salt, or its peroxide in the surface treatment agent B was controlled so that the adhesion amount of the second film formed by the surface treatment agent B was 4.0 g / m 2 , 8.0g / m 2 , 12g / m 2 .

[0112] As the surface treatment agent for forming a single film in Comparative Examples 1 to 4, the following surface treatment agents were used.

[0113] Surface treatment agent in Comparative Example 1: Surface treatment agent A of Examples 1 to 10.

[0114] Surface treatment agent in Comparative Example 2: Surface treatment agent A of Examples 11 to 19.

[0115] Surface treatment agent in Comparative Example 3: mineral oil (paraffin-based mineral oil, 8 cst (centistokes) at 40°C).

[0116] Surface treatment agent in Comparative Example 4: Surface treatment agent B of Examples 2 and 12

[0117] (1-3) Cleaning of metal materials

[0118] The surfaces of the metal materials used in the above-mentioned Examples and Comparative Examples were cleaned by the following method.

[0119] Use tap water to adjust the concentration of a commercially available degreaser (Fine Cleaner E6400, manufactured by Nippon Parkersei Co., Ltd.) to 20 g / L, and heat it to 60°C to maintain a constant temperature. Immerse the metal material in the above degreaser for 10 minutes to degrease. Subsequently, rinse off the remaining degreaser, dirt, etc. after immersing it in tap water at 25°C for 20 seconds. Next, immerse the washed metal material in 17.5% hydrochloric acid at 25°C for 10 minutes to remove dirt that cannot be removed by water washing. Furthermore, immerse it in tap water at 25°C for 20 seconds to wash off the hydrochloric acid attached to the metal material.

[0120] (1-4) Method for forming the first film and the second film of Examples 1 to 19

[0121] The first film and the second film were formed on the metal material subjected to the above cleaning treatment by the following method.

[0122] ·Examples 1 to 10

[0123] The cleaned metal material was immersed in the surface treatment agent A adjusted to 80°C for 10 minutes to form the first film. Subsequently, the metal material formed with the first film was immersed in tap water at 25°C for 30 seconds and washed with water. Table 1 shows the adhesion amount of the first film of Examples 1 to 10. The adhesion amount was calculated by measuring the weight of the metal material before and after the formation of the first film, taking the difference as the adhesion weight, and dividing it by the original surface area of ​​the metal material.

[0124] Furthermore, the metal material formed with the first film was immersed in a surface treatment agent B heated to 60°C for 15 seconds, taken out and naturally dried to form a second film, which was used as the metal material for plastic working of Examples 1 to 10. Table 1 shows the adhesion amount of the second film. The adhesion amount was calculated by measuring the weight of the metal material before and after the second film was formed, taking the difference as the adhesion weight, and dividing it by the surface area of ​​the original metal material.

[0125] ·Examples 11 to 19

[0126] The cleaned metal material was immersed in the surface treatment agent A adjusted to 90°C for 10 minutes to form the first film. Subsequently, the metal material formed with the first film was immersed in tap water at 25°C for 30 seconds to wash. Table 1 shows the adhesion amount of the first film of Examples 11 to 19. The adhesion amount was calculated by the same method as in Examples 1 to 10.

[0127] Furthermore, the metal material having the first film formed thereon was immersed in a surface treatment agent B heated to 60°C for 15 seconds, taken out, and then naturally dried to form a second film, which was used as the metal material for plastic working of Examples 11 to 19. Table 1 shows the adhesion amount of the second film of Examples 11 to 19. The adhesion amount was calculated by the same method as in Examples 1 to 10.

[0128] (1-5) Method for forming a single film of Comparative Examples 1 to 4

[0129] In Comparative Example 1, a single film was formed by the same method as the first film formation method in Examples 1 to 10, and then the metal material was immersed in tap water at 25° C. for 30 seconds and washed with water to obtain a metal material for plastic working of Comparative Example 1.

[0130] In Comparative Example 2, a single film was formed by the same method as the first film formation method in Examples 11 to 19, and then the metal material was immersed in tap water at 25° C. for 30 seconds and washed with water to obtain a metal material for plastic working of Comparative Example 2.

[0131] In Comparative Example 3, the sample was immersed in mineral oil heated to 40°C for 10 seconds and then taken out, and the excess mineral oil was wiped off to reduce the adhesion amount of the mineral oil (g / m2 ) becomes 4.0g / m 2 , as the metal material for plastic working of Comparative Example 3.

[0132] In Comparative Example 4, a single film was formed by the same method as the second film formation method in Examples 2 and 12, and then the metal material was immersed in tap water at 25° C. for 30 seconds and washed with water to obtain the metal material for plastic working of Comparative Example 4.

[0133] Table 1 shows the adhesion amounts of the single films of Comparative Examples 1 to 4.

[0134] (1-6) Evaluation test

[0135] (1-6-1) Ball reduction extrusion test

[0136] Evaluations of the weld resistance and lubricity were performed based on the ball reduction extrusion friction test method disclosed in the above reference.

[0137] The evaluation test was conducted as follows: After the film was formed, the protruding side portion of the barrel-shaped test piece was subjected to a diameter reduction extrusion process (intensive processing) using three spherical dies (SUJ-2 bearing balls with a diameter of 10 mm). The evaluation of the weld resistance of each test piece was based on Figure 1 The evaluation criteria shown (A is the best) were determined by visual inspection of the appearance of the second half of the diameter reduction extrusion process, in which the surface area was increased. The lubricity of each test piece was evaluated according to the following evaluation criteria.

[0138] In addition, in this example, there is no difference in corrosion resistance (comparison of rust conditions under equivalent environments) before and after plastic working. Therefore, it can be considered that the second film still remains after plastic working and protects the first film.

[0139] <Evaluation criteria for lubricity>

[0140] The lubricity was evaluated by comparing the maximum load value obtained during the diameter reduction extrusion process with the range of the maximum load value as the following evaluation standard. The smaller the maximum load value, the better the lubricity.

[0141] A: The maximum load value is less than 38kN.

[0142] B: The maximum load value is greater than 38kN and less than 40kN.

[0143] C: The maximum load value is greater than 40 kN and less than 42 kN.

[0144] D: Maximum load value is above 42kN.

[0145] [Table 1]

[0146] Table 1

[0147]

[0148] [Table 2]

[0149] Table 2

[0150]

[0151] Furthermore, although the present invention has been described in detail with reference to specific embodiments, it will be apparent to those skilled in the art that various changes and modifications can be made without departing from the spirit and scope of the present invention.

Claims

1. A metal material for plastic working, comprising a first film on a surface of the metal material or on the surface thereof, and a second film on a surface of the first film or on the surface thereof, The first film is a chemically synthesized film, The second membrane is a surface layer, The second film is formed only of a compound selected from ammonium salts, sodium salts, lithium salts and potassium salts of salicylic acid, ammonium salts, sodium salts, lithium salts and potassium salts of phthalic acid, and ammonium salts, sodium salts, lithium salts and potassium salts of benzoic acid.

2. The metal material for plastic working according to claim 1, wherein: The first film is a film containing at least one component selected from the group consisting of phosphates, oxalates, and aluminates.