Preparation method of NH2-MIL-101(Fe) / viscosity composite porous carbon material for dye adsorption
Through one-step in-situ synthesis and high-temperature calcination by solvothermal method, the preparation process of NH2-MIL-101(Fe)/viscose composite porous carbon materials is simplified, solving the problem of complex processes in the existing technology, and realizing the application of organic dyes. Efficient adsorption and material stability and adaptability, with environmental protection and saving characteristics.
Patent Information
- Application Number
- CN202310105369.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-02
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2043-02-02
AI Technical Summary
There is currently a lack of mature reaction system for preparing NH2-MIL-101(Fe)/viscose composite porous carbon materials, and the preparation process is complicated and difficult to operate.
The solvothermal method was used to synthesize NH2-MIL-101(Fe)/viscose composite nonwoven material in one step, and the NH2-MIL-101(Fe)/viscose composite porous carbon material was produced through high-temperature calcination in a tube furnace. Simplified process, reduce costs and improve adsorption performance.
It achieves efficient adsorption and removal of acidic or alkaline organic dyes. The material has good stability, strong adaptability, can be reused, and has the characteristics of environmental protection and saving.
Smart Images

Figure CN116212828B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of synthesis of functionally modified nonwoven materials of metal organic framework materials, and specifically is a method for preparing NH2-MIL-101 (Fe) / viscose composite porous carbon material for dye adsorption. Background Art
[0002] In recent years, organic dyes have been widely used in the industrial field, and the harm caused by the printing and dyeing wastewater to the ecological environment and human health is difficult to estimate. At present, the common methods for treating printing and dyeing wastewater include adsorption, biological methods, electrochemical treatment and photocatalytic technology. Among them, adsorption technology is widely used because of its low cost, wide application, simple operation, large adsorption capacity and high removal rate. Metal organic framework materials (MOFs) are crystalline porous materials with rich nanopore structures. They are formed by coordination self-assembly of central metal ions and organic ligands. They have the advantages of large specific surface area, high porosity, low density, adjustable pore size and designable structure. They have been widely used in adsorption, separation, energy storage, catalysis, biochemistry and drug sustained release. Among them, Fe in NH2-MIL-101(Fe) 3+ It has the advantages of high abundance, good stability, non-toxicity, and small band gap. Its structure has good stability in various organic solvents at room temperature for several months. Its mesoporous characteristics and large porous windows allow reactant molecules, such as organic dyes, to easily approach the active center. As a new adsorbent material, it has been used in gas separation and adsorption of pollutants in water, and is an ideal material for use as a wastewater dye adsorbent. Viscose spunlace nonwoven materials have abundant raw material sources, have a serrated skin-core structure and grooves, and have a certain adsorption capacity. In addition, since the carbon content of viscose fiber is as high as 44.4%, it is an excellent raw material for preparing carbon materials.
[0003] At present, there is no mature reaction system for the preparation of NH2-MIL-101(Fe) / viscosity composite porous carbon materials. There are generally problems such as complex process and difficult operation in the preparation process. Summary of the invention
[0004] The purpose of the present invention is to provide a method for preparing NH2-MIL-101 (Fe) / viscose composite porous carbon material for dye adsorption. In view of the defects of the existing preparation process, a solvent thermal method is used to synthesize NH2-MIL-101 (Fe) / viscose composite nonwoven material in one step, and then the NH2-MIL-101 (Fe) / viscose composite porous carbon material is obtained by high-temperature calcination in a tubular furnace. The method is simple in process. The base fabric and the raw materials for synthesizing Fe-based MOFs are put into a reactor together to obtain a composite material in one step, and then the adsorption performance can be improved by simple high-temperature calcination. The whole preparation process is simple, low in cost, and the experimental environment requirement is not high. The sample can be recycled and reused, which is environmentally friendly and economical.
[0005] In order to solve the above technical problems, the following technical solutions are adopted:
[0006] A method for preparing NH2-MIL-101(Fe) / viscosity composite porous carbon material for dye adsorption, characterized by comprising the following steps:
[0007] (1) Acidification and impregnation treatment of base fabric
[0008] (2) Preparation of reaction solution
[0009] A certain amount of ferric nitrate nonahydrate and 2-aminoterephthalic acid were completely dissolved in DMF solution, and then PVP was added, and magnetic stirring was performed at room temperature until it was completely dissolved, and the mixed solution was transferred to a PTFE reactor;
[0010] (3) Preparation of NH2-MIL-101(Fe) / viscose composite nonwoven materials
[0011] The impregnated viscose spunlace nonwoven fabric was placed vertically in a PTFE reactor containing the reaction solution, sealed, and reacted at high temperature in an oven. After the reaction was completed, it was naturally cooled to room temperature, washed alternately with ethanol and DMF, and dried in an oven under hot pressing to constant weight to obtain NH2-MIL-101(Fe) / viscose composite nonwoven material.
[0012] (4) Preparation of NH2-MIL-101(Fe) / viscosity composite porous carbon materials
[0013] The NH2-MIL-101(Fe) / viscose composite nonwoven material was placed in a tubular furnace and heated and kept warm for 1 hour to obtain the NH2-MIL-101(Fe) / viscose composite porous carbon material.
[0014] After optimization, the step (1) acidification: firstly, the viscose spunlace nonwoven material is heated and soaked in a dilute hydrochloric acid solution, then washed with deionized water, and dried at room temperature.
[0015] After optimization, the step (1) of impregnation is as follows: the acidified viscose spunlace nonwoven material is immersed in a mixed solution containing ferric nitrate nonahydrate and DMF for 30 minutes.
[0016] After optimization, the pH of the dilute hydrochloric acid in step (1) is 4.5 to 6.5, and the mixture is washed with deionized water until it becomes neutral.
[0017] After optimization, the feed ratio of ferric nitrate nonahydrate to DMF in step (1) is about 2.1-2.4:30-40, in units of g:mL.
[0018] Preferably, the magnetic stirring time in step (2) is 2 to 3 hours.
[0019] After optimization, the feed ratio of ferric nitrate nonahydrate, 2-aminoterephthalic acid, PVP and DMF in step (2) is about 2.1-2.4:0.8-1.1:0.3-0.6:30-40, in units of g:g:g:mL.
[0020] After optimization, the oven reaction temperature of step (3) is 130-150° C., and the reaction time is 15 h.
[0021] After optimization, the heating rate of the tubular furnace in step (4) is 2.5°C / min under a nitrogen atmosphere.
[0022] The above technical solution has the following beneficial effects:
[0023] The NH2-MIL-101(Fe) / viscose composite porous carbon material prepared by the present invention is used for adsorption and removal of different organic dyes in acidic or alkaline wastewater, and has different degrees of effect. Among them, the composite porous carbon material can achieve efficient adsorption of methylene blue dye at different water bath temperatures and pH values, and can be recycled and reused multiple times after adsorption, and has the characteristics of simple preparation method, low cost, and environmental friendliness. Therefore, the present invention proves that this composite material has good stability, strong adaptability, high dye removal efficiency, and good reusability, and has a broad application prospect.
[0024] The present invention adopts a solvent thermal method to synthesize NH2-MIL-101 (Fe) / viscose composite nonwoven material in one step, and then obtains NH2-MIL-101 (Fe) / viscose composite porous carbon material by high-temperature calcination in a tubular furnace. The method is simple in process, and the base fabric and the raw materials for synthesizing Fe-based MOFs are put into a reactor together to obtain a composite material in one step, and then the adsorption performance can be improved by simple high-temperature calcination. The whole preparation process is simple, the cost is low, the experimental environment requirement is not high, and the sample can be recycled and reused, which is environmentally friendly and economical.
[0025] Through a one-step in situ solvothermal method, Fe3+ It is evenly fixed on the viscose nonwoven material by complexing with amino groups to synthesize NH2-MIL-101(Fe) / viscose composite nonwoven material, and then calcined at high temperature to form a porous carbon structure in the composite material, thereby increasing the specific surface area of the composite material to obtain NH2-MIL-101(Fe) / viscose composite porous carbon material with high-efficiency adsorption performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] The present invention will be further described below in conjunction with the accompanying drawings:
[0027] Figure 1 This is a scanning electron microscope image of the NH2-MIL-101(Fe) / viscose composite nonwoven material before calcination;
[0028] Figure 2 It is a scanning electron microscope image of NH2-MIL-101(Fe) / viscose composite nonwoven material after calcination;
[0029] Figure 3 The adsorption efficiency of methylene blue on NH2-MIL-101(Fe) / viscosity composite porous carbon materials prepared at different calcination temperatures;
[0030] Figure 4 The adsorption efficiency of NH2-MIL-101(Fe) / viscosity composite porous carbon materials for different dyes
[0031] Figure 5 The adsorption efficiency of methylene blue at different water bath temperatures;
[0032] Figure 6 The adsorption efficiency of methylene blue at different pH values;
[0033] Figure 7 The adsorption efficiency of methylene blue after 5 cycles under the optimal adsorption conditions. DETAILED DESCRIPTION
[0034] The present invention adopts a solvent thermal method to synthesize NH2-MIL-101 (Fe) / viscose composite nonwoven material in one step, and then obtains NH2-MIL-101 (Fe) / viscose composite porous carbon material by high-temperature calcination in a tubular furnace. The method is simple in process, and the base fabric and the raw materials for synthesizing Fe-based MOFs are put into a reactor together to obtain a composite material in one step, and then the adsorption performance can be improved by simple high-temperature calcination. The whole preparation process is simple, the cost is low, the experimental environment requirement is not high, and the sample can be recycled and reused, which is environmentally friendly and economical.
[0035] The technical solution of the present invention is described in detail below in conjunction with specific embodiments and drawings:
[0036] Take a certain amount of viscose spunlace nonwoven material (2*2cm) and boil it in a dilute hydrochloric acid solution, then wash it with deionized water and dry it at room temperature. Dissolve 2.23g of ferric nitrate nine hydrate completely in 35mL of DMF solution to prepare an impregnation solution, and then soak the viscose nonwoven material treated with dilute acid in the impregnation solution for 30min. Dissolve 2.23g of ferric nitrate nine hydrate and 0.98g of 2-aminoterephthalic acid completely in 35mL of DMF solution. Then add 0.58g of PVP, stir magnetically for 1 to 2h at room temperature, and transfer the mixed solution to a PTFE reactor. Then, place the impregnated viscose nonwoven fabric vertically into the reactor, seal it, and react it in an oven at 150℃ for 15h. After the reaction is completed, cool it naturally to room temperature, wash it alternately with ethanol and DMF 3 times, and press dry it at 70℃ to constant weight to obtain NH2-MIL-101(Fe) / viscose composite nonwoven material.
[0037] The MOFs / viscose composite nonwoven material prepared above was dried in a vacuum oven at 70 °C for 1 h and then heated in a tube furnace at 2.5 °C·min -1 The temperature was raised at a rate of 200-350°C under nitrogen protection and kept warm for 1 h to obtain the porous carbon material NH2-MIL-101(Fe) / viscosity composite porous carbon material.
[0038] The surface morphology of the prepared NH2-MIL-101(Fe) / viscose composite nonwoven material and NH2-MIL-101(Fe) / viscose composite porous carbon material was observed using a scanning electron microscope JSM-5610LV. Figure 1 and Figure 2 ,from Figure 1 It can be seen that NH2-MIL-101(Fe) has a regular octahedral structure and is evenly fixed on the surface of the viscose spunlace nonwoven material. Figure 2 In the study, after carbonization at 300 °C, the surface of the NH2-MIL-101(Fe) / viscose composite porous carbon material still maintained the regular octahedral structure of NH2-MIL-101(Fe) with no significant change in morphology, while some tiny grooves and micropores appeared on the fiber surface of the viscose spunlace nonwoven material.
[0039] Accurately weigh the viscose spunlace nonwoven material, NH2-MIL-101(Fe) / viscose composite nonwoven material and NH2-MIL-101(Fe) / viscose composite porous carbon material prepared at different calcination temperatures, place them in a beaker, add 30 mL of a 50 mg / L methylene blue aqueous solution, and oscillate and adsorb in a water bath at 30°C in a dark environment. Take a certain amount of supernatant within a specific time, test its absorbance with a TU-1901 UV-visible photometer, and calculate its adsorption efficiency according to the following formula (1).
[0040]
[0041] The adsorption efficiency of NH2-MIL-101(Fe) / viscosity composite porous carbon materials prepared at different calcination temperatures is shown in Figure 2. Figure 3 As shown. It can be seen that compared with the viscose spunlace nonwoven material and the NH2-MIL-101(Fe) / viscose composite nonwoven material, the NH2-MIL-101(Fe) / viscose composite porous carbon material obtained after carbonization at 300°C can reach adsorption equilibrium in about 100 minutes when adsorbing methylene blue dye in water, and the adsorption efficiency reaches about 98%. This is due to the formation of a porous carbon structure after carbonization of the composite material, which increases its active site exposure and increases its contact area with the methylene blue dye.
[0042] Prepare aqueous solutions of methylene blue, rhodamine B, Congo red and acid orange II respectively, take 30 mL and place them in a water bath, then weigh a certain amount of NH2-MIL-101(Fe) / viscosity composite porous carbon material and place it in the beaker, shake and adsorb in a dark environment, take a certain amount of supernatant within a specific time, test its absorbance with a TU-1901 UV-visible photometer, and calculate its adsorption efficiency according to formula (1). The adsorption efficiency of the composite porous carbon material for different organic dyes is as follows: Figure 4 As shown, it can be seen that the adsorption efficiency of the composite material for alkaline methylene blue and rhodamine B dyes can reach more than 95%, and the adsorption efficiency for acidic Congo red and acid orange II is also more than 50%.
[0043] Accurately weigh a certain amount of NH2-MIL-101(Fe) / viscosity composite porous carbon material and place it in a beaker, add 30mL of 50mg / L methylene blue aqueous solution, then place it in a water bath at different temperatures (20℃~40℃), shake and adsorb in a dark environment, take a certain amount of supernatant at a specific time point, test its absorbance with a TU-1901 UV-visible photometer, and calculate its adsorption efficiency according to formula (1). The adsorption efficiency of the composite porous carbon material for methylene blue in water at different water bath temperatures is as follows: Figure 5As shown. It can be seen that the adsorption efficiency of the composite porous carbon material for methylene blue increases with the increase of the adsorption temperature. When the adsorption temperature is 30℃ and 40℃, the adsorption equilibrium efficiency is not much different. Considering that the higher the adsorption temperature, the higher the energy consumption, and it will also cause a certain degree of damage to the morphology of the composite material, the best water bath temperature in the adsorption process is 30℃. At this time, after reaching the adsorption equilibrium, its adsorption efficiency can reach about 98%.
[0044] Prepare 50 mg / L methylene blue aqueous solutions with pH = 3, 5, 7, 9 and 11 respectively, take 30 mL and place in the optimal water bath temperature (30 ° C), shake and adsorb in a dark environment, take a certain amount of supernatant within a specific time, test its absorbance with TU-1901 UV-visible photometer, and calculate its adsorption efficiency according to formula (1). The adsorption efficiency of methylene blue in water by composite porous carbon materials at different pH is as follows: Figure 6 As shown. It can be seen that the adsorption efficiency of the composite porous carbon material for methylene blue increases with the increase of pH value, and reaches the highest adsorption efficiency of 98% at pH = 9. This is attributed to the increase in the pH value of the methylene blue aqueous solution, which leads to an increase in the amount of negative charge on the surface of the NH2-MIL-101 (Fe) / viscose composite porous carbon material, which increases the electrostatic attraction between the negatively charged NH2-MIL-101 (Fe) / viscose composite porous carbon material and the positively charged methylene blue, thereby improving the adsorption efficiency of the material.
[0045] Anhydrous ethanol was selected as the desorbent. The NH2-MIL-101(Fe) / viscose composite porous carbon material that had adsorbed methylene blue was washed with anhydrous ethanol three times, then immersed in 150 ml of anhydrous ethanol until the desorption process was basically completed, and then hot-pressed and dried in a vacuum oven at 70°C for 6 hours, and then taken out for use. The dried NH2-MIL-101(Fe) / viscose composite porous carbon material was used as an adsorbent again to adsorb methylene blue in the water at the optimal water bath temperature and pH, and its absorbance was tested with a TU-1901 UV-visible photometer. This cycle was repeated 5 times, and the results of its repeated adsorption efficiency are shown in the figure. Figure 7 As shown in the figure, it can be seen that after five cycles, the adsorption efficiency of the adsorbent is still maintained above 86%, which shows that the structure and adsorption performance of the NH2-MIL-101(Fe) / viscosity composite porous carbon material used as an organic dye adsorbent are stable and can be used for multiple cycles.
[0046] The above are only specific embodiments of the present invention, but the technical features of the present invention are not limited thereto. Any simple changes, equivalent replacements or modifications made based on the present invention to solve basically the same technical problems and achieve basically the same technical effects are all included in the protection scope of the present invention.
Claims
1. A method for preparing NH2-MIL-101 (Fe) / viscosity composite porous carbon material for dye adsorption, characterized in that The steps include: (1) Acidification and impregnation treatment of base fabric First, the viscose spunlace nonwoven material is heated and soaked in a dilute hydrochloric acid solution with a pH of 4.5 to 6.5, then washed with deionized water until neutral, and dried at room temperature; the acidified viscose spunlace nonwoven material is immersed in a mixed solution containing ferric nitrate nonahydrate and DMF for 30 minutes; (2) Preparation of reaction solution A certain amount of ferric nitrate nonahydrate and 2-aminoterephthalic acid were completely dissolved in DMF solution, and then PVP was added, and magnetic stirring was performed at room temperature until it was completely dissolved, and the mixed solution was transferred to a PTFE reactor; (3) Preparation of NH2-MIL-101 (Fe) / viscose composite nonwoven materials The impregnated viscose spunlace nonwoven fabric is placed vertically into the PTFE reactor containing the mixed solution in step (2), sealed, and reacted at high temperature in an oven; after the reaction is completed, the fabric is naturally cooled to room temperature, washed alternately with ethanol and DMF, and dried in an oven under hot pressing until constant weight is obtained to obtain an NH2-MIL-101 (Fe) / viscose composite nonwoven material; (4) Preparation of NH2-MIL-101 (Fe) / viscosity composite porous carbon materials The NH2-MIL-101 (Fe) / viscose composite nonwoven material was placed in a tubular furnace and heated to 300°C under nitrogen protection and kept warm for 1 h to obtain NH2-MIL-101 (Fe) / viscose composite porous carbon material.
2. The method for preparing the NH2-MIL-101 (Fe) / viscosity composite porous carbon material for dye adsorption according to claim 1, characterized in that: In the step (1), the feed ratio of ferric nitrate nonahydrate to DMF is 2.1-2.4:30-40, in units of g:mL.
3. The method for preparing a NH2-MIL-101 (Fe) / viscosity composite porous carbon material for dye adsorption according to claim 1, characterized in that: The magnetic stirring time in step (2) is 2 to 3 hours.
4. The method for preparing the NH2-MIL-101 (Fe) / viscosity composite porous carbon material for dye adsorption according to claim 1, characterized in that: In the step (2), the feed ratio of ferric nitrate nonahydrate, 2-aminoterephthalic acid, PVP and DMF is 2.1-2.4:0.8-1.1:0.3-0.6:30-40, in units of g:g:g:mL.
5. The method for preparing a NH2-MIL-101 (Fe) / viscosity composite porous carbon material for dye adsorption according to claim 1, characterized in that: The oven reaction temperature in step (3) is 130-150° C., and the reaction time is 15 h.
6. The method for preparing a NH2-MIL-101 (Fe) / viscosity composite porous carbon material for dye adsorption according to claim 1, characterized in that: The heating rate of the tubular furnace in step (4) is 2.5°C / min under a nitrogen atmosphere.
Citation Information
Patent Citations
Preparation method and applications of porous composite material with peroxidase activity
CN105233869A
Preparation method and application of metal organic framework (MOF)-derived magnetic porous carbon material
CN110975808A
Preparation method and application of MIL-100 (Fe) / cellulose porous composite spheres
CN114672064A
Fe-MOFs-based magnetic charcoal composite adsorption material as well as preparation method and application thereof
CN115445566A
Preparation method for mofs photocatalytic material having high visible light response
WO2021258233A1