A method for preparing anhydrous formaldehyde

By using a high-entropy alloy catalyst to react with methanol in a fixed-bed reactor under specific conditions, the problems of high energy consumption and poor catalyst stability in the preparation of anhydrous formaldehyde in the existing technology are solved, and efficient generation of anhydrous formaldehyde and co-production of hydrogen are achieved effect.

CN116217359BActive Publication Date: 2024-10-25DALIAN INSTITUTE OF CHEMICAL PHYSICS CHINESE ACADEMY OF SCIENCES
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111477416.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-06
Publication Date
2024-10-25
Estimated Expiration
2041-12-06

AI Technical Summary

Technical Problem

The existing technology has the problems of high energy consumption, high cost and poor catalyst stability when preparing anhydrous formaldehyde, especially under high temperature conditions, the yield of formaldehyde is low and the selectivity is poor.

Method used

A high-entropy alloy catalyst is used to react with methanol in a fixed-bed reactor under specific temperature and pressure conditions. It is diluted with inert gas to generate anhydrous formaldehyde and co-produces hydrogen. The catalyst includes TiVMnFeCoZr and other components. Different carrier loads are prepared through spray drying and roasting. high-entropy alloy catalysts.

Benefits of technology

An efficient reaction to effectively generate anhydrous formaldehyde from methanol is achieved. The catalyst has good stability and the maximum yield can reach 83.2%. Hydrogen is produced in parallel, reducing the risk of equipment corrosion and distillation costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003393982580000121
    Figure BDA0003393982580000121
  • Figure BDA0003393982580000131
    Figure BDA0003393982580000131
Patent Text Reader

Abstract

The present invention relates to a method for preparing anhydrous formaldehyde, and more particularly to a method for synthesizing anhydrous formaldehyde by anaerobic dehydrogenation of methanol. The process is carried out in a fixed bed reactor, and methanol is directly dehydrogenated to prepare formaldehyde on a high entropy alloy catalyst under anaerobic conditions, and no water is produced during the reaction, so the produced formaldehyde is anhydrous formaldehyde, and hydrogen is co-produced at the same time.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for synthesizing anhydrous formaldehyde, in particular to a method for preparing anhydrous formaldehyde by dehydrogenation of formaldehyde under oxygen-free and inert conditions. Background Art

[0002] Formaldehyde is an important organic chemical raw material, which has been widely used in the production of many chemical products such as engineering plastics, urea-formaldehyde resin (urea-formaldehyde resin), phenolic resin, hexamethylenetetramine (urotropine), ethylene glycol, 1,4-butanediol, neopentyl glycol, pentaerythritol, trimethylolpropane and pyridine. At the same time, formaldehyde is also an important raw material for synthetic dyes, pesticides, fine and special chemicals, etc.

[0003] In recent years, with the increasing demand for anhydrous formaldehyde in downstream applications of formaldehyde, anhydrous formaldehyde is currently obtained by removing water from industrial formaldehyde aqueous solutions through various methods. At present, the industry generally uses methanol oxidation to prepare formaldehyde, usually on FeMoO catalysts at 300-450°C, or on Ag catalysts at 600-700°C. However, the formaldehyde prepared by this method contains a large amount of water, and the vapor pressure of formaldehyde aqueous solution is very low. Formaldehyde and water can easily form azeotropes, so the separation and purification of formaldehyde is very difficult, resulting in high energy consumption and high costs. In addition, the methanol oxidation process will cause over-oxidation to generate formic acid, which will corrode equipment.

[0004] The direct oxygen-free catalytic dehydrogenation of methanol to produce formaldehyde and byproduct hydrogen is easy to separate, does not require oxygen addition, and does not produce water, which can greatly save the investment and operating costs of distillation equipment; the corrosion problem of formic acid on equipment can also be effectively alleviated. The byproduct H2 can also be utilized, such as using it in the synthesis of raw material methanol, which can further improve the economy of the reaction process. Therefore, the direct oxygen-free dehydrogenation of methanol to produce anhydrous formaldehyde is an industrial process with great application prospects.

[0005] In recent years, a large number of studies have been conducted at home and abroad on the direct oxygen-free dehydrogenation of methanol to produce anhydrous formaldehyde. Methanol can be directly dehydrogenated to formaldehyde and hydrogen at high temperatures, but the formaldehyde yield is only 20% when the temperature is as high as 900°C. Moreover, as the temperature increases, although the methanol conversion rate increases, the formaldehyde selectivity decreases. Therefore, to obtain a high formaldehyde yield, the design and synthesis of the catalyst is the key. The catalysts reported so far are mainly divided into three categories: metal and oxide catalysts, alkali metal salt catalysts, and molecular sieve catalysts. Metal and oxide catalysts include metals such as Cu, Ag, and Zn and their oxides; alkali metal salt catalysts include oxides and carbonates, borates or molybdates of metals such as Li and Na; molecular sieve catalysts are mainly alkali metal or alkaline earth metal ZSM-5 molecular sieves, ZnO / all-silicon zeolite, etc. Only a small number of two-component alloys have been reported, such as TiFe alloys and CuZn alloys, which usually have high reaction temperatures (~600°C), low conversion rates, poor selectivity, and poor catalyst stability. The application of high entropy alloys in this reaction has not yet been reported.

[0006] This application intends to utilize the high temperature stability and high activity of high entropy alloys to catalyze the direct oxygen-free dehydrogenation of formaldehyde to produce anhydrous formaldehyde, which has important application value and scientific significance. Summary of the invention

[0007] The problem to be solved by the present invention is to provide a method for preparing anhydrous formaldehyde, starting from cheap, easily available and stable methanol, through an efficient high entropy alloy catalyst, to prepare anhydrous formaldehyde and simultaneously co-produce hydrogen.

[0008] The technical solution is:

[0009] In a fixed bed reactor, methanol is gasified and diluted with an inert gas or undiluted, and then reacts on a certain amount of high entropy alloy catalyst under certain temperature and pressure conditions to produce formaldehyde. No water is produced during the reaction, and hydrogen is co-produced.

[0010] The inert atmosphere includes: N2, Ar, He;

[0011] The inert gas accounts for 10-95% of the total volume of the total gas;

[0012] The mass space velocity of methanol on the catalyst is: 0.2-4h -1 ;

[0013] Reaction temperature: 400-650℃;

[0014] Reaction pressure: 0.5-5atm.

[0015] The inert atmosphere includes: N2;

[0016] The inert gas accounts for 30-80% of the total volume of the total gas;

[0017] The mass space velocity of methanol on the catalyst is: 0.5-4h -1 ;

[0018] Reaction temperature: 500-650℃;

[0019] Reaction pressure: 0.5-3atm.

[0020] The inert gas accounts for 50-70% of the total volume of the total gas;

[0021] The mass space velocity of methanol on the catalyst is: 1-3h -1 ;

[0022] Reaction temperature: 600-650℃;

[0023] The reaction pressure is: 0.5-1atm.

[0024] The high entropy alloy catalyst is a high entropy alloy with a body-centered cubic, face-centered cubic, hexagonal close-packed, or Laves-hexagonal close-packed structure.

[0025] The high entropy alloy catalyst is a high entropy alloy composed of TiVMnFeCoZr, a high entropy alloy composed of TiVCrMnFeZr, a high entropy alloy composed of TiCrMnFeNiZr, a high entropy alloy composed of TiVCrFeNiZr, a high entropy alloy composed of TiVZrNbHf, a high entropy alloy composed of TiVZrNbMo, a high entropy alloy composed of TiZrNbTa, a high entropy alloy composed of TiCrVNb, a high entropy alloy composed of MgTiFeCoNiZr, a high entropy alloy composed of AlCrMnFeNiW, a high entropy alloy composed of VMnFeNiLa, and a high entropy alloy composed of TiVCrFeCoZr;

[0026] The high entropy alloy catalyst also includes a catalyst carrier, and the carrier includes SiO2, Al2O3, SiC, and all-silicon zeolite.

[0027] The preparation method of the high entropy alloy catalyst is to dissolve the soluble salt of the metal corresponding to the high entropy alloy constituent element in a solvent, stir to form a uniform solution, then disperse the catalyst carrier therein to form a suspension, stir evenly, spray dry to obtain a solid powder, and then calcine and reduce at a certain temperature to obtain a high entropy alloy catalyst with different carrier loads.

[0028] The mass fraction of the catalyst carrier is 50-99%;

[0029] The solvent is one of water, ethanol and other soluble metal salts corresponding to the constituent elements of the high entropy alloy and their organic solvents or a mixture thereof;

[0030] The molar ratio of any two elements corresponding to the elements constituting the high entropy alloy is: 0.9 to 1.1;

[0031] The calcination temperature is 500-800°C;

[0032] The gas used in the roasting process is one of air or an inert gas containing 5-99.9% oxygen or a mixture thereof;

[0033] The reduction temperature is 600-900°C;

[0034] The atmosphere used in the reduction process contains H2, CO or other reducing gases or a mixture thereof; the reduction process may also contain N2, Ar, He or other inert gases or a mixture thereof, with the inert gas accounting for 30-95% of the volume of the total gas.

[0035] Beneficial technical effects

[0036] 1. The catalyst raw materials used in the present invention are cheap and readily available, the preparation process is controllable and easy to operate, and the effective reaction from methanol to anhydrous formaldehyde can be achieved;

[0037] 2. The catalyst has good stability, and the reaction process is simple, controllable and easy to operate. The highest yield of anhydrous formaldehyde can reach 83.2%, and hydrogen can also be co-produced. DETAILED DESCRIPTION

[0038] In order to further explain the present invention in detail, several specific implementation cases are given below, but the present invention is not limited to these embodiments.

[0039] Example 1

[0040] TiCl3 solution, ammonium metavanadate, Mn(NO3)2, Fe(NO3)3, Co(NO3)2 and ZrO(NO3)3 (the added amount is calculated according to the metal ion molar ratio of 0.9 / 1 / 1 / 1 / 1 / 1) are added to a deionized water solution, stirred to obtain a uniform solution, and then the carrier SiO2 is added (the added amount is 50% of the final sample mass), stirred to obtain a uniform suspension (with a solid mass content of 30%), spray dried to obtain a solid powder, and then calcined in an air atmosphere at 500°C for 24h and reduced in a hydrogen atmosphere at 600°C for 12h. The obtained sample is recorded as TiVMnFeCoZr / SiO2. X-ray diffraction (XRD) and transmission electron microscopy (TEM) characterizations show that the metal elements on the surface of the carrier are uniformly dispersed to form a Laves-hexagonal close-packed structure high entropy alloy.

[0041] The obtained sample was pressed into tablets with a size of 20-60 mesh, and then added into a fixed bed reactor. Methanol was introduced into the device after gasification. The inert dilution atmosphere was N2, and the volume of inert gas accounted for 10% of the total gas volume. The mass space velocity of methanol on the catalyst was 1h -1 The reaction was carried out at 600°C and 0.5 atm and monitored online by gas chromatography. The product yield and selectivity after 8 h of reaction are shown in Table 1.

[0042] Example 2 (using the catalyst sample in Example 1)

[0043] The obtained sample was pressed into tablets with a size of 20-60 mesh, and then added into a fixed bed reactor. Methanol was introduced into the device after gasification. The inert dilution atmosphere was N2, and the volume of inert gas accounted for 30% of the total gas volume. The mass space velocity of methanol on the catalyst was 1h -1 The reaction was carried out under the conditions of 600°C and 0.5 atm and monitored online by gas chromatography. The product yield and selectivity after 8 h of reaction are shown in Table 1.

[0044] Example 3 (using the catalyst sample in Example 1)

[0045] The obtained sample was pressed into tablets with a size of 20-60 mesh, and then added into a fixed bed reactor. Methanol was introduced into the device after gasification. The inert dilution atmosphere was N2, and the volume of inert gas accounted for 50% of the total gas volume. The mass space velocity of methanol on the catalyst was 1h -1 The reaction was carried out under the conditions of 600°C and 0.5 atm and monitored online by gas chromatography. The product yield and selectivity after 8 h of reaction are shown in Table 1.

[0046] Example 4 (using the catalyst sample in Example 1)

[0047] The obtained sample was pressed into tablets with a size of 20-60 mesh, and then added into a fixed bed reactor. Methanol was introduced into the device after gasification. The inert dilution atmosphere was N2, and the volume of inert gas accounted for 70% of the total gas volume. The mass space velocity of methanol on the catalyst was 1h -1 The reaction was carried out at 600°C and 0.5 atm and monitored online by gas chromatography. The product yield and selectivity after 8 h of reaction are shown in Table 1.

[0048] Example 5 (using the catalyst sample in Example 1)

[0049] The obtained sample was pressed into tablets with a size of 20-60 mesh, and then added into a fixed bed reactor. Methanol was introduced into the device after gasification. The inert dilution atmosphere was N2, and the volume of inert gas accounted for 95% of the total gas volume. The mass space velocity of methanol on the catalyst was 1h -1 The reaction was carried out at 600°C and 0.5 atm and monitored online by gas chromatography. The product yield and selectivity after 8 h of reaction are shown in Table 1.

[0050] Example 6

[0051] TiCl3 solution, ammonium metavanadate, Cr(NO3)3, Mn(NO3)2, Fe(NO3)3 and ZrO(NO3)3 (the added amount is calculated according to the metal ion molar ratio of 0.9 / 1 / 1 / 1 / 1 / 1.1) are added to a deionized water solution, stirred to obtain a uniform solution, and then the carrier Al2O3 (the added amount is 80% of the final sample mass) is added, stirred to obtain a uniform suspension (with a solid mass content of 30%), spray dried to obtain a solid powder, and then calcined at 800°C in a nitrogen atmosphere containing 5 vol% oxygen for 18 hours, and reduced at 900°C in a CO atmosphere for 6 hours. The obtained sample is recorded as TiVCrMnFeZr / Al2O3. X-ray diffraction (XRD) and transmission electron microscopy (TEM) characterizations show that the metal elements on the surface of the carrier are uniformly dispersed to form a Laves-hexagonal close-packed structure high entropy alloy.

[0052] The obtained sample was pressed into tablets with a size of 20-60 mesh, and then added into a fixed bed reactor. Methanol was introduced into the device after gasification. The inert dilution atmosphere was N2, and the volume of inert gas accounted for 60% of the total gas volume. The mass space velocity of methanol on the catalyst was 0.2h -1 The reaction was carried out at 650°C and 1 atm and monitored online by gas chromatography. The product yield and selectivity after 8 h of reaction are shown in Table 1.

[0053] Example 7 (using the catalyst sample in Example 6)

[0054] The obtained sample was pressed into tablets with a size of 20-60 mesh, and then added into a fixed bed reactor. Methanol was introduced into the device after gasification. The inert dilution atmosphere was N2, and the volume of inert gas accounted for 60% of the total gas volume. The mass space velocity of methanol on the catalyst was 0.5h -1 The reaction was carried out at 650°C and 1 atm and monitored online by gas chromatography. The product yield and selectivity after 8 h of reaction are shown in Table 1.

[0055] Example 8 (using the catalyst sample in Example 6)

[0056] The obtained sample was pressed into a 20-60 mesh size tablet and then added into a fixed bed reactor. Methanol was introduced into the device after gasification. The inert dilution atmosphere was N2, and the volume of inert gas accounted for 60% of the total gas volume. The mass space velocity of methanol on the catalyst was 1h -1 The reaction was carried out at 650°C and 1 atm and monitored online by gas chromatography. The product yield and selectivity after 8 h of reaction are shown in Table 1.

[0057] Example 9 (using the catalyst sample in Example 6)

[0058] The obtained sample was pressed into tablets with a mesh size of 20-60 and then added into a fixed bed reactor. Methanol was introduced into the device after gasification. The inert dilution atmosphere was N2, and the volume of inert gas accounted for 60% of the total gas volume. The mass space velocity of methanol on the catalyst was 3h -1 The reaction was carried out at 650°C and 1 atm and monitored online by gas chromatography. The product yield and selectivity after 8 h of reaction are shown in Table 1.

[0059] Example 10 (using the catalyst sample in Example 6)

[0060] The obtained sample was pressed into tablets with a size of 20-60 mesh, and then added into a fixed bed reactor. Methanol was introduced into the device after gasification. The inert dilution atmosphere was N2, and the volume of inert gas accounted for 60% of the total gas volume. The mass space velocity of methanol on the catalyst was 4h -1 The reaction was carried out at 650°C and 1 atm and monitored online by gas chromatography. The product yield and selectivity after 8 h of reaction are shown in Table 1.

[0061] Embodiment 11

[0062] TiCl3 solution, Cr(NO3)3, Mn(NO3)2, Fe(NO3)3, Ni(NO3)2 and ZrO(NO3)3 (the added amount is calculated according to the metal ion molar ratio of 1 / 1 / 1 / 1 / 1 / 1) are added to a deionized water solution, stirred to obtain a uniform solution, and then a carrier SiC is added (the added amount is 90% of the final sample mass), stirred to obtain a uniform suspension (of which the solid mass content is 50%), spray dried to obtain a solid powder, and then calcined at 700°C in a nitrogen atmosphere containing 60 vol% oxygen for 12 hours, and reduced at 800°C in a 30 vol% hydrogen-argon mixed atmosphere for 24 hours. The obtained sample is recorded as TiCrMnFeNiZr / SiC. X-ray diffraction (XRD) and transmission electron microscopy (TEM) characterizations show that the metal elements on the surface of the carrier are uniformly dispersed to form a Laves-hexagonal close-packed structure high entropy alloy.

[0063] The obtained sample was pressed into tablets with a size of 20-60 mesh, and then added into a fixed bed reactor. Methanol was introduced into the device after gasification. The inert dilution atmosphere was He, and the volume of inert gas accounted for 60% of the total gas volume. The mass space velocity of methanol on the catalyst was 0.5h -1 The reaction was carried out at 400°C and 1 atm and monitored online by gas chromatography. The product yield and selectivity after 8 h of reaction are shown in Table 1.

[0064] Example 12 (using the catalyst sample in Example 11)

[0065] The obtained sample was pressed into tablets with a size of 20-60 mesh, and then added into a fixed bed reactor. Methanol was introduced into the device after gasification. The inert dilution atmosphere was He, and the volume of inert gas accounted for 60% of the total gas volume. The mass space velocity of methanol on the catalyst was 0.5h -1 The reaction was carried out at 500°C and 1 atm and monitored online by gas chromatography. The product yield and selectivity after 8 h of reaction are shown in Table 1.

[0066] Example 13 (using the catalyst sample in Example 11)

[0067] The obtained sample was pressed into tablets with a size of 20-60 mesh, and then added into a fixed bed reactor. Methanol was introduced into the device after gasification. The inert dilution atmosphere was He, and the volume of inert gas accounted for 60% of the total gas volume. The mass space velocity of methanol on the catalyst was 0.5h -1 The reaction was carried out at 600°C and 1 atm and monitored online by gas chromatography. The product yield and selectivity after 8 h of reaction are shown in Table 1.

[0068] Example 14 (using the catalyst sample in Example 11)

[0069] The obtained sample was pressed into tablets with a size of 20-60 mesh, and then added into a fixed bed reactor. Methanol was introduced into the device after gasification. The inert dilution atmosphere was He, and the volume of inert gas accounted for 60% of the total gas volume. The mass space velocity of methanol on the catalyst was 0.5h -1 The reaction was carried out at 650°C and 1 atm and monitored online by gas chromatography. The product yield and selectivity after 8 h of reaction are shown in Table 1.

[0070] Embodiment 15

[0071] TiCl3 solution, ammonium metavanadate, Cr(NO3)3, Fe(NO3)3, Ni(NO3)2 and ZrO(NO3)3 (the added amount is calculated according to the metal ion molar ratio of 1 / 1 / 1 / 1 / 1 / 1) are added to the deionized water solution, stirred to obtain a uniform solution, and then the carrier all-silicon zeolite (the added amount is 80% of the final sample mass) is added, stirred to obtain a uniform suspension (wherein the solid mass content is 50%), spray dried to obtain a solid powder, and then calcined at 700℃ in a nitrogen atmosphere containing 99.9vol% oxygen for 12h, and reduced at 800℃ in a mixed atmosphere of 50vol% hydrogen and CO for 8h. The obtained sample is recorded as TiVCrFeNiZr / all-silicon zeolite. X-ray diffraction (XRD) and transmission electron microscopy (TEM) characterizations show that the metal elements on the surface of the carrier are uniformly dispersed to form a Laves-hexagonal close-packed structure high entropy alloy.

[0072] The obtained sample was pressed into tablets with a size of 20-60 mesh, and then added into a fixed bed reactor. Methanol was introduced into the device after gasification. The inert dilution atmosphere was Ar, and the volume of inert gas accounted for 60% of the total gas volume. The mass space velocity of methanol on the catalyst was 0.5h -1 The reaction was carried out at 600°C and 0.5 atm and monitored online by gas chromatography. The product yield and selectivity after 8 h of reaction are shown in Table 1.

[0073] Example 16 (using the catalyst sample in Example 15)

[0074] The obtained sample was pressed into tablets with a size of 20-60 mesh, and then added into a fixed bed reactor. Methanol was introduced into the device after gasification. The inert dilution atmosphere was Ar, and the volume of inert gas accounted for 60% of the total gas volume. The mass space velocity of methanol on the catalyst was 0.5h -1 The reaction was carried out at 600°C and 1 atm and monitored online by gas chromatography. The product yield and selectivity after 8 h of reaction are shown in Table 1.

[0075] Example 17 (using the catalyst sample in Example 15)

[0076] The obtained sample was pressed into tablets with a size of 20-60 mesh, and then added into a fixed bed reactor. Methanol was introduced into the device after gasification. The inert dilution atmosphere was Ar, and the volume of inert gas accounted for 60% of the total gas volume. The mass space velocity of methanol on the catalyst was 0.5h -1 The reaction was carried out at 600°C and 3 atm and monitored online by gas chromatography. The product yield and selectivity after 8 h of reaction are shown in Table 1.

[0077] Example 18 (using the catalyst sample in Example 15)

[0078] The obtained sample was pressed into tablets with a size of 20-60 mesh, and then added into a fixed bed reactor. Methanol was introduced into the device after gasification. The inert dilution atmosphere was Ar, and the volume of inert gas accounted for 60% of the total gas volume. The mass space velocity of methanol on the catalyst was 0.5h -1 The reaction was carried out at 600°C and 5 atm and monitored online by gas chromatography. The product yield and selectivity after 8 h of reaction are shown in Table 1.

[0079] Embodiment 19

[0080] TiCl3 solution, ammonium metavanadate, ZrO(NO3)3, ammonium niobium oxalate and hafnium oxynitrate (the added amount is calculated according to the metal ion molar ratio of 1 / 1 / 1 / 1 / 1) are added to a mixed solution of deionized water and acetonitrile (volume ratio 1 / 1), stirred to obtain a uniform solution, and then the carrier SiO2 (the added amount is 70% of the final sample mass) is added, stirred to obtain a uniform suspension (with a solid mass content of 50%), spray dried to obtain a solid powder, and then calcined in an air atmosphere at 700°C for 10h, and reduced at 800°C in a mixed atmosphere of 95vol% CO and He for 8h. The obtained sample is recorded as TiVZrNbHf / SiO2. X-ray diffraction (XRD) and transmission electron microscopy (TEM) characterization show that the metal elements on the surface of the carrier are uniformly dispersed to form a body-centered cubic structure high entropy alloy.

[0081] The obtained sample was pressed into a 20-60 mesh size tablet and then added into a fixed bed reactor. Methanol was introduced into the device after gasification. The inert dilution atmosphere was N2, and the volume of inert gas accounted for 60% of the total gas volume. The mass space velocity of methanol on the catalyst was 1h -1 The reaction was carried out at 600°C and 1 atm and monitored online by gas chromatography. The product yield and selectivity after 8 h of reaction are shown in Table 1.

[0082] Embodiment 20

[0083] TiCl3 solution, ammonium metavanadate, ZrO(NO3)3, ammonium niobium oxalate and ammonium molybdate (the added amount is calculated according to the metal ion molar ratio of 1 / 1 / 1 / 1 / 1) are added to deionized water, stirred to obtain a uniform solution, and then the carrier SiO2 is added (the added amount is 70% of the final sample mass), stirred to obtain a uniform suspension (wherein the solid mass content is 70%), spray dried to obtain a solid powder, and then calcined in an air atmosphere at 700℃ for 10h, and reduced in a mixed atmosphere of 30vol% H2 and Ar at 800℃ for 24h. The obtained sample is recorded as TiVZrNbMo / SiO2. X-ray diffraction (XRD) and transmission electron microscopy (TEM) characterization show that the metal elements on the surface of the carrier are uniformly dispersed to form a face-centered cubic structure high entropy alloy.

[0084] The obtained sample was pressed into a 20-60 mesh size tablet and then added into a fixed bed reactor. Methanol was introduced into the device after gasification. The inert dilution atmosphere was N2, and the volume of inert gas accounted for 60% of the total gas volume. The mass space velocity of methanol on the catalyst was 1h -1 The reaction was carried out at 600°C and 1 atm and monitored online by gas chromatography. The product yield and selectivity after 8 h of reaction are shown in Table 1.

[0085] Embodiment 21

[0086] TiCl3 solution, ZrO(NO3)3, ammonium niobium oxalate and ammonium molybdate (the added amount is calculated according to the metal ion molar ratio of 1 / 1 / 1 / 1) are added to anhydrous ethanol, stirred to obtain a uniform solution, and then the carrier SiO2 (the added amount is 70% of the final sample mass) is added, stirred to obtain a uniform suspension (wherein the solid mass content is 70%), spray dried to obtain a solid powder, and then calcined in an air atmosphere at 700℃ for 10h, and reduced in a mixed atmosphere of 30vol% H2 and N2 at 800℃ for 24h. The obtained sample is recorded as TiZrNbTa / SiO2. X-ray diffraction (XRD) and transmission electron microscopy (TEM) characterization show that the metal elements on the surface of the carrier are uniformly dispersed to form a body-centered cubic structure high entropy alloy.

[0087] The obtained sample was pressed into a 20-60 mesh size tablet and then added into a fixed bed reactor. Methanol was introduced into the device after gasification. The inert dilution atmosphere was N2, and the volume of inert gas accounted for 60% of the total gas volume. The mass space velocity of methanol on the catalyst was 1h -1 The reaction was carried out at 600°C and 1 atm and monitored online by gas chromatography. The product yield and selectivity after 8 h of reaction are shown in Table 1.

[0088] Embodiment 22

[0089] TiCl3 solution, Cr(NO3)3, ammonium metavanadate and ammonium niobium oxalate (the added amount is calculated according to the metal ion molar ratio of 1 / 1 / 1 / 1) are added to a mixed solution of deionized water and ethanol (volume ratio 5 / 1), stirred to obtain a uniform solution, and then the carrier SiO2 (the added amount is 70% of the final sample mass) is added, stirred to obtain a uniform suspension (with a solid mass content of 50%), spray dried to obtain a solid powder, and then calcined in an air atmosphere at 700°C for 10h, and reduced in a mixed atmosphere of 30vol% H2 and N2 at 800°C for 24h. The obtained sample is recorded as TiCrVNb / SiO2. X-ray diffraction (XRD) and transmission electron microscopy (TEM) characterization show that the metal elements on the surface of the carrier are uniformly dispersed to form a body-centered cubic structure high entropy alloy.

[0090] The obtained sample was pressed into a 20-60 mesh size tablet and then added into a fixed bed reactor. Methanol was introduced into the device after gasification. The inert dilution atmosphere was N2, and the volume of inert gas accounted for 60% of the total gas volume. The mass space velocity of methanol on the catalyst was 1h -1 The reaction was carried out at 600°C and 1 atm and monitored online by gas chromatography. The product yield and selectivity after 8 h of reaction are shown in Table 1.

[0091] Embodiment 23

[0092] Mg(NO3)2, TiCl3 solution, Fe(NO3)3, Co(NO3)2, Ni(NO3)2, and ZrO(NO3)3 (the added amount is calculated according to the metal ion molar ratio of 1 / 1 / 1 / 1 / 1 / 1) are added to deionized water, stirred to obtain a uniform solution, and then the carrier Al2O3 is added (the added amount is 70% of the final sample mass), stirred to obtain a uniform suspension (with a solid mass content of 50%), spray dried to obtain a solid powder, and then calcined in an air atmosphere at 700°C for 10h, and reduced in a mixed atmosphere of 30vol% H2 and N2 at 800°C for 24h. The obtained sample is recorded as MgTiFeCoNiZr / Al2O3. X-ray diffraction (XRD) and transmission electron microscopy (TEM) characterizations show that the metal elements on the surface of the carrier are uniformly dispersed to form a body-centered cubic structure high entropy alloy.

[0093] The obtained sample was pressed into a 20-60 mesh size tablet and then added into a fixed bed reactor. Methanol was introduced into the device after gasification. The inert dilution atmosphere was N2, and the volume of inert gas accounted for 60% of the total gas volume. The mass space velocity of methanol on the catalyst was 1h -1 The reaction was carried out at 600°C and 1 atm and monitored online by gas chromatography. The product yield and selectivity after 8 h of reaction are shown in Table 1.

[0094] Embodiment 24

[0095] Al(NO3)3, Cr(NO3)3, Mn(NO3)2, Fe(NO3)3, Ni(NO3)2, and ammonium tungstate (the added amount is calculated according to the metal ion molar ratio of 1 / 1 / 1 / 1 / 1 / 1) are added to deionized water, stirred to obtain a uniform solution, and then the carrier Al2O3 (the added amount is 70% of the final sample mass) is added, stirred to obtain a uniform suspension (with a solid mass content of 50%), spray dried to obtain a solid powder, and then calcined in an air atmosphere at 700°C for 10h, and reduced in a mixed atmosphere of 30vol% H2 and N2 at 800°C for 24h. The obtained sample is recorded as AlCrMnFeNiW / Al2O3. X-ray diffraction (XRD) and transmission electron microscopy (TEM) characterizations show that the metal elements on the surface of the carrier are uniformly dispersed to form a body-centered cubic structure high entropy alloy.

[0096] The obtained sample was pressed into a 20-60 mesh size tablet and then added into a fixed bed reactor. Methanol was introduced into the device after gasification. The inert dilution atmosphere was N2, and the volume of inert gas accounted for 60% of the total gas volume. The mass space velocity of methanol on the catalyst was 1h -1 The reaction was carried out at 600°C and 1 atm and monitored online by gas chromatography. The product yield and selectivity after 24 h of reaction are shown in Table 1.

[0097] Embodiment 25

[0098] Add ammonium metavanadate, Mn(NO3)2, Fe(NO3)3, Ni(NO3)2, and La(NO3)3 (the added amount is calculated according to the metal ion molar ratio of 1 / 1 / 1 / 1 / 1) to deionized water, stir to obtain a uniform solution, then add the carrier Al2O3 (the added amount is 70% of the final sample mass), stir to obtain a uniform suspension (with a solid mass content of 50%), spray dry to obtain a solid powder, then calcine in an air atmosphere at 700℃ for 10h, and reduce in a mixed atmosphere of 30vol% H2 and N2 at 800℃ for 24h. The obtained sample is recorded as VMnFeNiLa / Al2O3. X-ray diffraction (XRD) and transmission electron microscopy (TEM) characterization show that the metal elements on the surface of the carrier are uniformly dispersed to form a body-centered cubic structure high entropy alloy.

[0099] The obtained sample was pressed into a 20-60 mesh size tablet and then added into a fixed bed reactor. Methanol was introduced into the device after gasification. The inert dilution atmosphere was N2, and the volume of inert gas accounted for 60% of the total gas volume. The mass space velocity of methanol on the catalyst was 1h -1 The reaction was carried out at 600°C and 1 atm and monitored online by gas chromatography. The product yield and selectivity after 36 h of reaction are shown in Table 1.

[0100] Embodiment 26

[0101] TiCl3 solution, ammonium metavanadate, Cr(NO3)3, Fe(NO3)3, Co(NO3)2, and ZrO(NO3)2 (the added amount is calculated according to the metal ion molar ratio of 1 / 1 / 1 / 1 / 1 / 1) are added to deionized water, stirred to obtain a uniform solution, and then the carrier Al2O3 (the added amount is 99% of the final sample mass) is added, stirred to obtain a uniform suspension (with a solid mass content of 50%), spray dried to obtain a solid powder, and then calcined in an air atmosphere at 700°C for 10h, and reduced at 800°C in a mixed atmosphere of 30vol% H2 and N2 for 24h. The obtained sample is recorded as TiVCrFeCoZr / Al2O3. X-ray diffraction (XRD) and transmission electron microscopy (TEM) characterizations show that the metal elements on the surface of the carrier are uniformly dispersed to form a hexagonal close-packed high entropy alloy.

[0102] The obtained sample was pressed into a 20-60 mesh size tablet and then added into a fixed bed reactor. Methanol was introduced into the device after gasification. The inert dilution atmosphere was N2, and the volume of inert gas accounted for 60% of the total gas volume. The mass space velocity of methanol on the catalyst was 1h -1 The reaction was carried out at 600°C and 1 atm and monitored online by gas chromatography. The product yield and selectivity after 72 h of reaction are shown in Table 1.

[0103] Comparative Example 1

[0104] TiCl3 solution was added to a mixed solution of deionized water and ethanol (volume ratio 5 / 1), stirred to obtain a uniform solution, then carrier SiO2 (the amount added was 70% of the final sample mass), stirred to obtain a uniform suspension (with a solid mass content of 50%), spray dried to obtain a solid powder, then calcined at 700°C in an air atmosphere for 10 hours, and reduced at 800°C in a 30 vol% H2 and N2 mixed atmosphere for 24 hours. The obtained sample was recorded as Ti / SiO2.

[0105] The obtained sample was pressed into a 20-60 mesh size tablet and then added into a fixed bed reactor. Methanol was introduced into the device after gasification. The inert dilution atmosphere was N2, and the volume of inert gas accounted for 60% of the total gas volume. The mass space velocity of methanol on the catalyst was 1h -1 The reaction was carried out at 600°C and 1 atm and monitored online by gas chromatography. The product yield and selectivity after 8 h of reaction are shown in Table 1.

[0106] Comparative Example 2

[0107] TiCl3 solution and Cr(NO3)3 (the amount added is calculated according to the metal ion molar ratio of 1 / 1) are added to a mixed solution of deionized water and ethanol (volume ratio 5 / 1), stirred to obtain a uniform solution, and then the carrier SiO2 (the amount added is 70% of the final sample mass) is added, stirred to obtain a uniform suspension (with a solid mass content of 50%), spray dried to obtain a solid powder, and then calcined in an air atmosphere at 700°C for 10h, and reduced in a mixed atmosphere of 30vol% H2 and N2 at 800°C for 24h. The obtained sample is recorded as TiCr / SiO2. X-ray diffraction (XRD) and transmission electron microscopy (TEM) characterization show that the metal elements on the carrier surface are unevenly dispersed and no specific structural alloy is formed.

[0108] The obtained sample was pressed into a 20-60 mesh size tablet and then added into a fixed bed reactor. Methanol was introduced into the device after gasification. The inert dilution atmosphere was N2, and the volume of inert gas accounted for 60% of the total gas volume. The mass space velocity of methanol on the catalyst was 1h -1 The reaction was carried out at 600°C and 1 atm and monitored online by gas chromatography. The product yield and selectivity after 8 h of reaction are shown in Table 1.

[0109] Comparative Example 3

[0110] TiCl3 solution, Cr(NO3)3, and ammonium niobium oxalate (the added amount is calculated according to the metal ion molar ratio of 1 / 1 / 1) are added to a mixed solution of deionized water and ethanol (volume ratio 5 / 1), stirred to obtain a uniform solution, and then the carrier SiO2 (the added amount is 70% of the final sample mass) is added, stirred to obtain a uniform suspension (with a solid mass content of 50%), spray dried to obtain a solid powder, and then calcined in an air atmosphere at 700°C for 10 hours, and reduced in a mixed atmosphere of 30vol% H2 and N2 at 800°C for 24 hours. The obtained sample is recorded as TiCrNb / SiO2. X-ray diffraction (XRD) and transmission electron microscopy (TEM) characterization show that the metal elements on the carrier surface are unevenly dispersed and no specific structural alloy is formed.

[0111] The obtained sample was pressed into a 20-60 mesh size tablet and then added into a fixed bed reactor. Methanol was introduced into the device after gasification. The inert dilution atmosphere was N2, and the volume of inert gas accounted for 60% of the total gas volume. The mass space velocity of methanol on the catalyst was 1h -1 The reaction was carried out at 600°C and 1 atm and monitored online by gas chromatography. The product yield and selectivity after 8 h of reaction are shown in Table 1.

[0112] Comparative Example 4

[0113] Add magnesium carbonate, titanium sulfate, iron nitrate, copper nitrate and zinc nitrate to deionized water (the amount added is calculated according to the metal ion molar ratio of 1 / 1 / 1 / 1 / 1), stir to obtain a uniform solution, then add the carrier Al2O3 (the amount added is 70% of the final sample mass), stir to obtain a uniform suspension (wherein the solid mass content is 50%), spray dry to obtain a solid powder, then roast in 700℃ air atmosphere for 10h, and reduce in 800℃ 30vol% H2 and N2 mixed atmosphere for 24h. The obtained sample is recorded as MgTiFeCuZn / Al2O3, and the XRD (X-ray diffraction) and TEM (transmission electron microscopy) characterization results show that Mg, Ti, Fe, Cu, and Zn cannot form a uniformly dispersed high entropy alloy.

[0114] The obtained sample was pressed into a 20-60 mesh size tablet and then added into a fixed bed reactor. Methanol was introduced into the device after gasification. The inert dilution atmosphere was N2, and the volume of inert gas accounted for 60% of the total gas volume. The mass space velocity of methanol on the catalyst was 1h -1 The reaction was carried out at 600°C and 1 atm and monitored online by gas chromatography. The product yield and selectivity after 8 h of reaction are shown in Table 1.

[0115] Comparative Example 5

[0116] Sodium carbonate, magnesium carbonate, cobalt nitrate, nickel nitrate and copper nitrate were added to deionized water (the amount added was calculated according to the metal ion molar ratio of 1 / 1 / 1 / 1 / 1), stirred to obtain a uniform solution, and then the carrier Al2O3 (the amount added was 70% of the final sample mass) was added, stirred to obtain a uniform suspension (wherein the solid mass content was 50%), spray dried to obtain a solid powder, and then calcined in an air atmosphere at 700℃ for 10h, and reduced in a mixed atmosphere of 30vol% H2 and N2 at 800℃ for 24h. The obtained sample was recorded as NaMgCoNiCu / Al2O3, and the XRD and TEM characterization results showed that Na, Mg, Co, Ni, and Cu could not form a uniformly dispersed high entropy alloy.

[0117] The obtained sample was pressed into a 20-60 mesh size tablet and then added into a fixed bed reactor. Methanol was introduced into the device after gasification. The inert dilution atmosphere was N2, and the volume of inert gas accounted for 60% of the total gas volume. The mass space velocity of methanol on the catalyst was 1h -1 The reaction was carried out at 600°C and 1 atm and monitored online by gas chromatography. The product yield and selectivity after 8 h of reaction are shown in Table 1.

[0118] Comparative Example 6

[0119] Titanium sulfate, manganese nitrate, iron nitrate, tin nitrate and antimony acetate were added to deionized water (the amount added was calculated according to the metal ion molar ratio of 1 / 1 / 1 / 1 / 1), stirred to obtain a uniform solution, and then the carrier Al2O3 (the amount added was 70% of the final sample mass) was added, stirred to obtain a uniform suspension (wherein the solid mass content was 50%), spray dried to obtain a solid powder, and then calcined in an air atmosphere at 700℃ for 10h, and reduced in a mixed atmosphere of 30vol% H2 and N2 at 800℃ for 24h. The obtained sample was recorded as TiMnFeSnSb / Al2O3, and the XRD and TEM characterization results showed that Ti, Mn, Fe, Sn, and Sb could not form a uniformly dispersed high entropy alloy.

[0120] The obtained sample was pressed into a 20-60 mesh size tablet and then added into a fixed bed reactor. Methanol was introduced into the device after gasification. The inert dilution atmosphere was N2, and the volume of inert gas accounted for 60% of the total gas volume. The mass space velocity of methanol on the catalyst was 1h -1 The reaction was carried out at 600°C and 1 atm and monitored online by gas chromatography. The product yield and selectivity after 8 h of reaction are shown in Table 1.

[0121] Table 1 Reaction evaluation results

[0122]

[0123]

[0124] From Examples 1-5, it can be seen that the higher the volume ratio of the inert gas, the higher the methanol conversion rate, but the selectivity is slightly reduced. Considering the reaction efficiency, it is more appropriate to select an inert gas volume ratio of 50-70%. From Examples 6-10, it can be seen that the higher the mass space velocity of methanol, the lower the conversion rate and the lower the selectivity. From Examples 11-14, it can be seen that the higher the reaction temperature, the higher the conversion rate, the lower the selectivity, and the suitable temperature range is 600-650°C. . From Examples 15-18, it can be seen that the higher the reaction pressure, the lower the conversion rate, and the selectivity is also reduced. The suitable range is 0.5-1atm. From Comparative Examples 1-3 and Example 22, it can be seen that the catalytic activity of a single active component, a two-component alloy and a three-component alloy is not as good as that of a high entropy alloy catalyst. From Comparative Examples 4-6, it can be seen that a multi-component metal mixture of other element combinations cannot form a high entropy alloy with a specific crystal structure. It is a mixture of simple metals or partial element alloys, and its catalytic performance is poor.

Claims

1. A method for catalytically preparing anhydrous formaldehyde, characterized in that: In a fixed bed reactor, methanol is gasified and, after being diluted with an inert gas or not, reacts on a high entropy alloy catalyst of a selected element combination to generate formaldehyde. No water is produced during the reaction, and hydrogen is co-produced at the same time. The high entropy alloy is one or more of a high entropy alloy composed of TiVMnFeCoZr, a high entropy alloy composed of TiVCrMnFeZr, a high entropy alloy composed of TiCrMnFeNiZr, a high entropy alloy composed of TiVCrFeNiZr, a high entropy alloy composed of TiVZrNbHf, a high entropy alloy composed of TiVZrNbMo, a high entropy alloy composed of TiZrNbTa, a high entropy alloy composed of TiCrVNb, a high entropy alloy composed of MgTiFeCoNiZr, a high entropy alloy composed of AlCrMnFeNiW, a high entropy alloy composed of VMnFeNiLa, and a high entropy alloy composed of TiVCrFeCoZr, wherein the combination of the selected elements is a determined combination; The inert atmosphere includes: one or more of N2, Ar, and He; The inert gas accounts for 10-95% of the total volume of the total gas, wherein the total gas is methanol and the inert gas; The mass space velocity of methanol on the high entropy alloy catalyst is: 0.2-4 h -1 ; Reaction temperature: 400-650 ℃; Reaction pressure: 0.5-5 atm; The preparation method of the high entropy alloy catalyst is as follows: dissolving a soluble salt of a metal corresponding to a constituent element of the high entropy alloy in a solvent, stirring to form a uniform solution, then dispersing a catalyst carrier therein to form a suspension, stirring evenly, spray drying to obtain a solid powder, and then calcining and reducing to obtain a high entropy alloy catalyst loaded with different carriers; Alternatively, a soluble salt of a metal corresponding to a high entropy alloy constituent element is dissolved in a solvent, stirred to form a uniform solution, spray-dried to obtain a solid powder, and then calcined and reduced to obtain a non-supported high entropy alloy catalyst.

2. The method according to claim 1, characterized in that: The inert atmosphere includes: N2; The inert gas accounts for 30-80% of the total volume of the total gas; The mass space velocity of methanol on the high entropy alloy catalyst is: 0.5-4 h -1 ; Reaction temperature: 500-650 ℃; Reaction pressure: 0.5-3 atm.

3. The method according to claim 1 or 2, characterized in that: The inert gas accounts for 50-70% of the total volume of the total gas; The mass space velocity of methanol on the high entropy alloy catalyst is: 1-3 h -1 ; Reaction temperature: 600-650 ℃; Reaction pressure: 0.5-1 atm.

4. The method according to claim 1, characterized in that: The high entropy alloy catalyst is a high entropy alloy having one or more of body-centered cubic, face-centered cubic, hexagonal close-packed and Laves-hexagonal close-packed structures.

5. The method according to claim 1 or 4, characterized in that: The high entropy alloy catalyst also includes a catalyst carrier, which includes one or more of SiO2, Al2O3, SiC, and all-silicon zeolite. The high entropy alloy is loaded on the carrier, and the mass fraction of the catalyst carrier is 50-99%.

6. The method according to claim 1, characterized in that: The solvent is: water, ethanol, other soluble high entropy alloy constituent elements corresponding to the metal soluble salt and its organic solvent, or a mixture of two or more thereof; The molar ratio between any two elements corresponding to the elements constituting the high entropy alloy is: 0.9-1.1; The calcination temperature is 500-800°C and the time is more than 2 hours; The gas used in the roasting process is one of air and / or an inert gas containing 5-99.9% oxygen by volume or a mixture thereof; the inert gas comprises one or a mixture of two or more of N2, Ar, He or other gases; The reduction temperature is 600-900°C; The atmosphere used in the reduction process contains one or two of H2 and CO, or a mixture of one or two of H2 and CO and one or more of other reducing gases; the reducing gas in the reduction process may also contain a mixture of one or more of N2, Ar, He or other inert gases, with the inert gas accounting for 30-95% of the volume of the total gas.

7. The method according to claim 6, characterized in that: The molar ratio between any two elements corresponding to the elements constituting the high entropy alloy is: 0.93-1.07; The calcination temperature is 600-800°C and the calcination time is 8-24 h. The reduction temperature is 700-800°C.