An isocyanate polymerization catalyst and a preparation method thereof, and a method for removing isocyanate impurities in an organic solvent
By using an isocyanate polymerization catalyst combined with a Ce(P204)3/MHPO4/AlR3 catalyst and a modified alumina carrier, the problem of difficult removal of isocyanate impurities in the solvent system is solved, and the long-term stable operation of the device and increased output during the isocyanate production process are achieved. .
Patent Information
- Application Number
- CN202111459262.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-12-02
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2041-12-02
AI Technical Summary
In the current technology, it is difficult to effectively remove impurities in the solvent system during the isocyanate production process, resulting in device blockage and poor production stability, which affects long-term operation and economic benefits.
An isocyanate polymerization catalyst containing active components and a carrier is used, combined with a modified alumina carrier through the Ce(P204)3/MHPO4/AlR3 catalyst, to catalyze the polymerization reaction of isocyanate, reduce the degree of polymerization of isocyanate, and reduce the accumulation of impurities. , and achieve effective removal of impurities through distillation and incineration.
It effectively reduces the accumulation of isocyanate impurities in the solvent system, extends the stable operation cycle of the device, reduces the frequency of shutdowns and maintenance, increases output, and reduces the replacement of fresh solvent, bringing economic benefits.
Smart Images

Figure CN116217856B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of preparing isocyanates by phosgenation, and in particular to a catalyst for removing isocyanates from organic solvents, and a method for removing impurities from organic solvents in the production process of isocyanates. Background Art
[0002] Isocyanate is a general term for various esters of isocyanic acid. It is an important raw material for the production of polyurethane and is widely used in coatings, adhesives, foams, leather, elastomers and other fields. According to structural classification, isocyanates are divided into aliphatic, alicyclic and aromatic isocyanates. The production methods of isocyanates are classified into phosgenation and non-phosgenation according to different raw materials. The phosgenation production process is mature and economically reasonable. It is the main method for industrial production of isocyanates today. 85%-90% of aliphatic isocyanates are produced by phosgenation.
[0003] The phosgene method is divided into liquid phase phosgenation and gas phase phosgenation. In 1989, Bayer first used gas phase phosgenation to produce aliphatic isocyanates, which has the advantages of low phosgene dosage, high yield, and fast reaction speed. In the gas phase phosgenation method, the raw material amine is first gasified and sent to a mixing reactor together with phosgene to react at 200-600°C to prepare isocyanates; the liquid phase phosgenation method is divided into cold reaction and hot reaction. In the cold reaction process, amines and phosgene generate carbamoyl chloride under low temperature conditions, and in the hot reaction process, carbamoyl chloride is decomposed to obtain isocyanate and HCl. Aliphatic isocyanates have low yields and difficult process development. They are also known as the jewel in the crown of the isocyanate industry. The reaction process temperature is high, and the raw materials and products are easily broken to produce small molecular isocyanates that enter the solvent circulation system and accumulate continuously. With the accumulation of small molecular isocyanates, the concentration increases and is easy to react to generate solid coke, causing the pipelines, heat exchangers and other equipment in the solvent circulation system to be blocked, ultimately affecting the long-term stable operation of production. Therefore, the production stability of aliphatic isocyanate is often poor. It is difficult for the industry to produce continuously for more than half a year. Maintenance affects production by 10 to 20 days, affecting tens of millions of economic benefits. Therefore, it is necessary to study methods to reduce the impurity content in the system and improve the stability of device operation.
[0004] CN110724029A discloses a recovery and purification device and process for o-dichlorobenzene, a solvent for photochemical reaction. The process of producing TDI by liquid phase phosgene method produces impurities such as carbon tetrachloride. This method uses a distillation tower to remove carbon tetrachloride from the solvent o-dichlorobenzene, and at the same time obtains a relatively pure solvent. The built-in design of the reboiler significantly reduces the high-temperature residence time of the material in the tower, and minimizes the generation of by-products. If this method is used to remove isocyanates in the solvent system, due to the strong activity of isocyanates, they are easily blocked by reaction or crystallization during the enrichment and removal process, and long-term operation is difficult.
[0005] CN111825573A discloses a method for purifying p-phenylene diisocyanate, which uses an aromatic hydrocarbon solvent to dissolve p-phenylene diisocyanate, adds activated carbon to adsorb impurities, and cools and purifies the p-phenylene diisocyanate product to obtain a high-quality product with white color and neat appearance. This method mainly removes impurities through activated carbon adsorption. Activated carbon itself has many impurities and needs additional purification. In addition, the difference in the adsorption capacity of different activated carbons for small molecular isocyanates has not been demonstrated in detail, and its use has limitations.
[0006] A catalyst for preparing polyisocyanate composition is disclosed in CN109749036A, which is an imine type quaternary ammonium salt catalyst, which is mainly for preparing trimerization and polymer of low color, and in downstream application. Therefore, its catalytic activity is relatively low, and in the continuous production process, it is necessary to use a large device to ensure the residence time, and there are certain limitations. And the catalyst application range is isocyanate monomer, and acid is relatively low, and acidity is relatively strong in the solvent system, which has a poisonous effect on the catalyst, and this also limits the application of most isocyanate trimerization and polymerized catalyst in the solvent system. Therefore, it is necessary to find a high-efficiency catalyst suitable for the solvent system. Summary of the invention
[0007] The purpose of the present invention is to provide a new catalyst and reaction removal method for removing impurities from the solvent in the production process of isocyanate, so as to overcome the defects of the above-mentioned prior art, remove impurities in the solvent system, reduce blockages in the production equipment, extend the stable operation cycle of the system, and increase production.
[0008] To achieve the above object, the technical solution of the present invention is as follows:
[0009] An isocyanate polymerization catalyst comprises an active component and a carrier, and specifically comprises the following components:
[0010]
[0011] The composition of the carrier includes:
[0012] ZrO2 20wt%-60wt%,
[0013] Al2O3 40wt%-80wt%.
[0014] A method for preparing an isocyanate polymerization catalyst comprises the following steps:
[0015] a. Mix Ce2O3, water and concentrated hydrochloric acid to completely dissolve Ce2O3 and evaporate until crystals are precipitated. Cool and crystallize. Add water to the resulting crystals and filter out the insoluble matter.
[0016] b. Configure P 204and ethanol, dropwise adding the mixed solution into the aqueous solution prepared in a, and adding the modified alumina carrier;
[0017] c. Add ammonia water to the mixture obtained in b, precipitate and layer, filter and dry to obtain the loaded Ce (P 204 )3 solid catalyst;
[0018] d. Ce after load (P 204 )3 catalyst and 0.5-2wt% MHPO4 aqueous solution were impregnated, aged, and dried to obtain Ce(P 204 )3 / MHPO4 solid catalyst;
[0019] e、Ce(P 204 )3 / MHPO4 solid catalyst was mixed with co-catalyst AlR3, aged and dried to obtain supported Ce(P 204 )3 / MHPO4 / AlR3 catalyst.
[0020] In step a of the present invention, the mass ratio of Ce2O3 to concentrated hydrochloric acid is 2:5 to 4:5, and the mass ratio of water to concentrated hydrochloric acid is 1:1 to 3:1.
[0021] In step b of the present invention, the dropping temperature is controlled to be maintained at 0-50°C, preferably 25°C.
[0022] In step b of the present invention, P 204 The mass ratio of the dosage to ethanol is 1:1 to 1:4, P 204 The mass ratio to Ce2O3 is 6:1 to 16:1.
[0023] In step b of the present invention, the mass ratio of the carrier to Ce2O3 is 100:1 to 500:1.
[0024] In step c of the present invention, the concentration of ammonia water is in the range of 10% to 28%, and it is added dropwise until the pH value of the solution is 6 to 7. The temperature of the process is controlled at about 25°C.
[0025] In step d of the present invention, the mass ratio of the MHPO4 aqueous solution to Ce2O3 is 100:1 to 500:1; the aging time is 3h to 10h, preferably 4 to 5h.
[0026] The MHPO4 described in the present invention includes but is not limited to alkali metal phosphates such as MgHPO4, CaHPO4, and Na2HPO4, preferably MgHPO4.
[0027] In step e of the present invention, the Ce(P 204The mass ratio of )3 / MHPO4 solid catalyst to AlR3 is 1:0.5 to 1:3, the aging temperature is 20 to 60°C, and the aging time is 1h to 10h, preferably 3 to 5h.
[0028] The AlR3 described in the present invention, wherein R = alkyl groups such as -CH3, -CH2CH3, -CH2CH2CH3, etc.
[0029] The method for preparing the carrier of the present invention comprises the following steps:
[0030] (1) Mixing a soluble zirconium salt, γ-alumina and water to form a slurry, and adjusting the pH to 3.0 to 7.0 using aqueous ammonia;
[0031] (2) Aging for 1-2 hours and drying to obtain a zirconium oxide-coated modified γ-alumina carrier.
[0032] The soluble zirconium salt of the present invention includes but is not limited to zirconyl sulfate, zirconium chloride, zirconium phosphate, etc., preferably zirconyl sulfate.
[0033] In step (1) of the present invention, the weight ratio of the soluble zirconium salt to the γ-type alumina is 1:1 to 1:10, preferably 1:5 to 4:5.
[0034] In step (1) of the present invention, the water content in the slurry is 10wt% to 20wt%.
[0035] In step (1) of the present invention, the concentration of the aqueous ammonia is 10wt% to 20wt%.
[0036] The catalyst support possesses sufficient strength to avoid breakdown of particle-particle or wall-particle forces during long term use. This enables the catalyst to operate in harsh environments such as high acidity, high pressure and high temperature in hydrogenation or other processing of biomass derived oxygenate feeds.
[0037] The second aspect of the present invention provides use of the catalyst in removing isocyanate impurities in a solvent.
[0038] A method for removing isocyanate impurities from an organic solvent in an isocyanate production process comprises the following steps:
[0039] A mixed solution containing isocyanate, organic solvent and liquid phosgene in an isocyanate production system is subjected to a catalytic reaction in a reactor loaded with the catalyst of the present invention, and the isocyanate is polymerized by the catalytic reaction to generate an isocyanate polymer, which is then distilled and purified, and the light component liquid phase at the top of the tower is used to obtain a purified organic solvent with impurities removed, and the heavy component liquid phase at the bottom of the tower is discharged and incinerated.
[0040] The catalyst can efficiently catalyze the polymerization of isocyanate, wherein Ce(P 204)3 plays a major catalytic role, the monomer is inserted between the Ce-polymer bonds, and the steric hindrance of the ligand inhibits the back-biting reaction of the polymer chain end, reduces dimerization and trimerization, and then highly polymerizes to become a heavy component.
[0041] Alkyl aluminum as a co-catalyst, with Ce(P 204 )3 to form a coordination reaction to form a rare earth metal ion alkyl bond. The greater the steric hindrance of the alkyl group, the higher the catalytic activity. Hydrogen phosphate is used as the second co-catalyst. Hydrogen phosphate reacts with Ce(P 204 )3 forms a complex system and produces a synergistic effect. Due to the presence of -OH in the hydrogen phosphate group, the high polymerization of isocyanate is effectively inhibited, and the reaction obtains a polymer with a molecular weight of less than 10,000, preventing the distillation process from being blocked by excessive viscosity.
[0042] Anionic catalyst systems generally initiate isocyanate polymerization at very low temperatures (below -50°C), while the catalyst system prepared in the present invention can catalyze the polymerization of aliphatic isocyanates in a wide temperature range (-50 to 50°C).
[0043] The aliphatic isocyanate includes but is not limited to HDI, HMDI, IPDI, XDI, etc., and the catalyst also has a catalytic effect on non-aliphatic isocyanates including MDI, TDI, PI, etc.
[0044] In the impurity removal method of the present invention, the organic solvent includes one or more of benzene, toluene, xylene, chlorobenzene, o-dichlorobenzene, p-dichlorobenzene, monochlorobiphenyl, dialkyl terephthalate and diethyl phthalate, preferably chlorobenzene.
[0045] In the impurity removal method of the present invention, a mixed solution containing isocyanate, organic solvent and liquid phosgene in the isocyanate production process is passed into a catalytic decomposition reactor for catalytic reaction to obtain a liquid phase containing phosgene, trace isocyanate, isocyanate polymer heavy components and organic solvent. Subsequently, the liquid phase enters a distillation tower for distillation, separation and purification, the light components of the liquid phase at the top of the tower are collected to obtain the purified organic solvent, and the heavy component liquid phase at the bottom of the tower is discharged and incinerated.
[0046] The isocyanate content in the mixed solution containing isocyanate, organic solvent and liquid phosgene of the present invention is about 0.1% to 5%, preferably 0.5% to 1.0%.
[0047] In the impurity removal method of the present invention, the catalyst volume space velocity range is 0.5-6h -1 , preferably 1.0-2.0 h -1 .
[0048] In the impurity removal method of the present invention, the reaction temperature is 10-50°C, preferably 20-30°C, and the pressure is 0.1-0.3Mpa(a), preferably 0.1-0.2Mpa(a).
[0049] The isocyanate monomer content in the liquid phase after catalytic self-polymerization is less than 2000 ppm, preferably within 1000 ppm.
[0050] The beneficial effects of the present invention are:
[0051] (1) After using this process, isocyanate impurities in the solvent circulation system can be effectively removed, effectively reducing the risk of impurity self-polymerization and blockage in the system, achieving long-term stable operation of the solvent system, reducing the frequency of unplanned shutdowns and thereby increasing production, and avoiding tens of millions of economic losses caused by shutdowns and maintenance.
[0052] (2) It can effectively solve the problem of isocyanate impurity enrichment in the solvent system, reduce or eliminate the hundreds of tons of fresh solvent replacement in the solvent system, is green and environmentally friendly, and has considerable economic benefits. The incineration of the heavy component impurities generated can bring economic benefits of hundreds of thousands of yuan. BRIEF DESCRIPTION OF THE DRAWINGS
[0053] Figure 1 1 is a schematic diagram of the process flow of Example 4, wherein 1 is a mixed solution, 2 is a catalytic reactor, 3 is a treated mixed solution, 4 is an organic solvent after purification, 5 is a liquid phase of heavy components in the bottom of the tower, and 6 is a non-condensable gas. DETAILED DESCRIPTION
[0054] The following examples will further illustrate the method provided by the present invention, but the present invention is not limited to the listed examples, and should also include any other known changes within the scope of the claims of the present invention.
[0055] Gas chromatography
[0056] Detector: Agilent 7890B gas chromatograph
[0057] The isocyanate content detection method is carried out in accordance with GB / T 30431-2020 General method for laboratory gas chromatograph.
[0058] Particle strength determination method
[0059] Detector: KC-4 digital particle strength tester
[0060] The particle strength test methods are carried out in accordance with the wear resistance and compressive strength methods in Part 3 of "GB / T 30202.3.-2013 Test Methods for Coal-Based Activated Carbon for Desulfurization and Denitrification".
[0061] Vector preparation:
[0062] (1) Weighing 300 g of zirconium chloride and γ-alumina in a weight ratio of 1:2, adding deionized water based on 10 wt % of the obtained slurry and stirring to prepare a slurry, adding ammonia water to the slurry to adjust the pH to 7, and the ammonia concentration is 10 wt %;
[0063] (2) The pH value was controlled at 7, aged for about 2 hours, and vacuum dried to obtain a modified γ-alumina carrier.
[0064] Example 1 Preparation of Catalyst A:
[0065] a. Take a 2000mL flask, add 2.1g rare earth oxide Ce2O3, 12mL distilled water and 4mL concentrated hydrochloric acid in sequence, heat to completely dissolve Ce2O3 and evaporate until crystals are about to precipitate, cool and crystallize, add 25mL distilled water, filter out insoluble matter, and then add about 50mL distilled water.
[0066] b. Configure 25g P 204 and 75 mL of ethanol, add dropwise the rare earth chloride aqueous solution prepared in step a, and at the same time add 900 g of modified γ alumina carrier.
[0067] c. Add 10% ammonia water to control the pH to 6-7, stir and let stand to allow the solution to precipitate and separate into layers, decant and filter, collect the solid, and dry in vacuo.
[0068] d. The product obtained in step c was immersed in 400 g of 0.5 wt% MgHPO4 aqueous solution, aged for 5 h, and dried at 120° C. to obtain Ce(P 204 )3 / MgHPO4 solid catalyst.
[0069] e. Add 15 g of triethylaluminum to the product obtained in step d, age it at 50° C. for 5 h, and vacuum dry it for 12 h to obtain Ce(P 204 )3 / MgHPO4 / Al(C2H5)3 rare earth catalyst.
[0070] Example 2 Preparation of Catalyst B
[0071] a. Take a 2000mL flask, add 3.5g rare earth oxide Ce2O3, 12mL distilled water and 5mL concentrated hydrochloric acid in sequence, heat to completely dissolve Ce2O3 and evaporate until crystals are about to precipitate, cool and crystallize, add 40mL distilled water, filter out insoluble matter, and then add about 80mL distilled water.
[0072] b. Configure 40g P 204 and 80 mL of ethanol, dropwise add the rare earth chloride aqueous solution prepared in step a, and at the same time add 900 g of modified γ alumina carrier.
[0073] c. Add 10% ammonia water to control the pH to 6-7, stir and let stand to allow the solution to precipitate and separate into layers, decant and filter, collect the solid, and dry in vacuo.
[0074] d. The product obtained in step c was immersed in 400 g of 1 wt% MgHPO4 aqueous solution, aged for 4 h, and dried at 120° C. to obtain Ce(P 204 )3 / MgHPO4 solid catalyst.
[0075] e. Add 30 g of triethylaluminum to the product obtained in step d, age it at 50° C. for 5 h, and vacuum dry it for 12 h to obtain Ce(P 204 )3 / MgHPO4 / Al(C2H5)3 rare earth catalyst.
[0076] Example 3 Preparation of Catalyst C
[0077] a. Take a 2000mL flask, add 3.5g rare earth oxide Ce2O3, 12mL distilled water and 5mL concentrated hydrochloric acid in sequence, heat to completely dissolve Ce2O3 and evaporate until crystals are about to precipitate, cool and crystallize, add 30mL distilled water, filter out insoluble matter, and then add about 100mL distilled water.
[0078] b. Configure 35g P 204 and 80 mL of ethanol, dropwise add the rare earth chloride aqueous solution prepared in step a, and at the same time add 900 g of modified γ alumina carrier.
[0079] c. Add 10% ammonia water to control the pH to 6-7, stir and let stand to allow the solution to precipitate and separate into layers, decant and filter, collect the solid, and dry in vacuo.
[0080] d. The product obtained in step c was immersed in 400 g of 1 wt% CaHPO4 aqueous solution, aged for 5 h, and dried at 120° C. to obtain Ce(P 204 )3 / CaHPO4 solid catalyst.
[0081] e. Add 20 g of triethylaluminum to the product obtained in step d, age it at 50° C. for 5 h, and vacuum dry it for 12 h to obtain Ce(P 204 )3 / CaHPO4 / Al(C2H5)3 rare earth catalyst.
[0082] Comparative Example 1 Preparation of Catalyst D
[0083] a. Take a 2000mL flask, add 2.1g rare earth oxide Ce2O3, 12mL distilled water and 4mL concentrated hydrochloric acid in sequence, heat to completely dissolve Ce2O3 and evaporate until crystals are about to precipitate, cool and crystallize, add 25mL distilled water, filter out insoluble matter, and then add about 100mL distilled water.
[0084] b. Configure 25g P 204 and 80 mL of ethanol, the rare earth chloride aqueous solution prepared in step a was added dropwise, and 900 g of unmodified γ-alumina carrier was added at the same time.
[0085] c. Add 10% ammonia water to control the pH to 6-7, stir and let stand to allow the solution to precipitate and separate into layers, decant and filter, collect the solid, and dry in vacuo.
[0086] d. The product obtained in step c was immersed in 400 g of 0.5 wt% MgHPO4 aqueous solution, aged for 5 h, and dried at 120° C. to obtain Ce(P 204 )3 / MgHPO4 solid catalyst.
[0087] e. Add 15 g of triethylaluminum to the product obtained in step d, age it at 50° C. for 5 h, and vacuum dry it for 12 h to obtain Ce(P 204 )3 / MgHPO4 / Al(C2H5)3 rare earth catalyst.
[0088] Comparative Example 2 Preparation of Catalyst E
[0089] a. Take a 2000mL flask, add 2.1g rare earth oxide Ce2O3, 12mL distilled water and 4mL concentrated hydrochloric acid in sequence, heat to completely dissolve Ce2O3 and evaporate until crystals are about to precipitate, cool and crystallize, add 50mL distilled water, filter out insoluble matter, and then add about 100mL distilled water.
[0090] b. Configure 25g P 204 and 80 mL of ethanol, dropwise add the rare earth chloride aqueous solution prepared in step a, and at the same time add 900 g of modified γ alumina carrier.
[0091] c. Add 10% ammonia water to control the pH to 6-7, stir and let stand to allow the solution to precipitate and separate into layers, decant and filter, collect the solid, and dry in vacuo.
[0092] d. The product obtained in step c was immersed in 400 g of 0.5 wt% MgHPO4 aqueous solution, aged for 5 h, and dried at 120° C. to obtain Ce(P 204 )3 / MgHPO4 solid catalyst.
[0093] e. Add 5 g of triethylaluminum to the product obtained in step d, age it at 50° C. for 5 h, and vacuum dry it for 12 h to obtain Ce(P 204 )3 / MgHPO4 / Al(C2H5)3 rare earth catalyst.
[0094] Comparative Example 3 Preparation of Catalyst F
[0095] a. Take a 2000mL flask, add 2.1g rare earth oxide Ce2O3, 12mL distilled water and 4mL concentrated hydrochloric acid in sequence, heat to completely dissolve Ce2O3 and evaporate until crystals are about to precipitate, cool and crystallize, add 30mL distilled water, filter out insoluble matter, and then add about 50mL distilled water.
[0096] b. Configure 25g P 204 and 80 mL of ethanol, dropwise add the rare earth chloride aqueous solution prepared in step a, and at the same time add 900 g of modified γ alumina carrier.
[0097] c. Add 10% ammonia water to control the pH to 6-7, stir and let stand to allow the solution to precipitate and separate into layers, decant and filter, collect the solid, and dry in vacuo.
[0098] d. The product obtained in step c was immersed in 20 g of 1 wt% MgHPO4 aqueous solution, aged for 5 h, and dried at 120° C. to obtain Ce(P 204 )3 / MgHPO4 solid catalyst.
[0099] e. Add 15 g of triethylaluminum to the product obtained in step d, age it at 50° C. for 5 h, and vacuum dry it for 12 h to obtain Ce(P 204 )3 / MgHPO4 / Al(C2H5)3 rare earth catalyst.
[0100] Comparative Example 4 Preparation of Catalyst G
[0101] a. Take a 2000mL flask, add 2.1g rare earth oxide Ce2O3, 12mL distilled water and 4mL concentrated hydrochloric acid in sequence, heat to completely dissolve Ce2O3 and evaporate until crystals are about to precipitate, cool and crystallize, add 30mL distilled water, filter out insoluble matter, and then add about 50mL distilled water.
[0102] b. Configure 5g P 204 and 60 mL of ethanol, dropwise add the prepared rare earth chloride aqueous solution, and at the same time add 900 g of modified γ alumina carrier.
[0103] c. Add 10% ammonia water to control the pH to 6-7, stir and let stand to allow the solution to precipitate and separate into layers, decant and filter, collect the solid, and dry in vacuo.
[0104] d. The product obtained in step c was immersed in 400 g of 0.5 wt% MgHPO4 aqueous solution, aged for 5 h, and dried at 120° C. to obtain Ce(P 204 )3 / MgHPO4 solid catalyst.
[0105] e. Add 15 g of triethylaluminum to the product obtained in step d, age it at 50° C. for 5 h, and vacuum dry it for 12 h to obtain Ce(P204 )3 / MgHPO4 / Al(C2H5)3 rare earth catalyst.
[0106] Application Examples
[0107] A mixed solution 1 containing 1wt% HDI, 98wt% chlorobenzene, 0.5wt% liquid phosgene, and 0.5wt% HCl enters the catalytic reactor 2 through the bottom of the reactor at a flow rate of 5kg / h. The catalytic reactor 2 is filled with a catalyst. The reactor size is 120mm*250mm, the catalyst filling amount is 2.4L, and the catalyst volume space velocity is 1.9h -1 , at about 20°C and 0.1 MPa (a) pressure conditions, catalytic polymerization of isocyanate is carried out, and after the reaction, a mixed solution 3 containing phosgene, trace isocyanate, isocyanate polymer heavy components, organic solvent, and trace HCl is obtained. The content of isocyanate monomer in the mixed solution after catalysis is shown in Table 1. After distillation treatment, the top liquid phase obtains a purified organic solvent 4, and the isocyanate monomer in the solvent is shown in Table 1. The heavy component liquid phase 5 in the bottom of the tower is discharged and incinerated, and non-condensable gases such as hydrogen chloride 6 enter the alkali solution absorption tower.
[0108] The statistical results of each catalyst treatment are shown in Table 1.
[0109] Table 1 Isocyanate removal rate results of each catalyst
[0110]
[0111]
[0112] Summary of experimental results of embodiments and comparative examples:
[0113] Through the experiments of the above embodiments and comparative examples, it is found that an organic solvent containing impurities in the production process of aliphatic isocyanate can effectively reduce the isocyanate impurity content in the solvent after passing through a catalytic decomposition reactor, greatly reducing the risk of equipment clogging due to isocyanate self-polymerization, improving the long-term stable operation of the device, and increasing production; at the same time, the self-metabolism of impurities in the solvent system is realized, and no additional fresh solvent replacement is required, which is green and environmentally friendly. The addition of two co-catalysts greatly improves the catalytic activity, and the generated polymerized isocyanate will not form a high-viscosity substance during the distillation process to block the equipment, and can operate for a long time.
[0114] The embodiments of the present invention have been described above, and the above description is exemplary, not exhaustive, and is not limited to the disclosed embodiments. Many modifications and changes will be apparent to those skilled in the art without departing from the scope and spirit of the described embodiments.
Claims
1. An isocyanate polymerization catalyst comprising the following components: The composition of the carrier includes: ZrO2 20wt%-60wt%, Al2O3 40wt%-80wt%; The MHPO4 is selected from one or more of MgHPO4, CaHPO4, and Na2HPO4; The AlR3, wherein R=-CH3, -CH2CH3, -CH2CH2CH3.
2. A method for preparing the isocyanate polymerization catalyst according to claim 1, comprising the following steps: a. Mix Ce2O3, water and concentrated hydrochloric acid to completely dissolve Ce2O3 and evaporate until crystals are precipitated. Cool and crystallize. Add water to the resulting crystals and filter out the insoluble matter. b. Configure P 204 and ethanol mixed solution, add dropwise to the aqueous solution prepared in a, and add a carrier; c. Add ammonia water to the mixture obtained in b, precipitate and layer, filter and dry to obtain the loaded Ce (P 204 )3 solid catalyst; d. Ce after load (P 204 )3 catalyst and 0.5-2wt% MHPO4 aqueous solution were impregnated, aged, and dried to obtain Ce(P 204 )3 / MHPO4 solid catalyst; e、Ce(P 204 )3 / MHPO4 solid catalyst was mixed with co-catalyst AlR3, aged and dried to obtain supported Ce(P 204 )3 / MHPO4 / AlR3 catalyst.
3. The method according to claim 2, characterized in that In the step b, P 204 The mass ratio to Ce2O3 is 6:1 to 16:
1.
4. The method according to claim 2, characterized in that: In the step b, the mass ratio of the carrier to Ce2O3 is 100:1 to 500:
1.
5. The method according to claim 2, characterized in that: In the step d, the mass ratio of the MHPO4 aqueous solution to Ce2O3 is 100:1 to 500:
1.
6. The method according to claim 2, characterized in that In the step e, the Ce(P 204 The mass ratio of )3 / MHPO4 solid catalyst to AlR3 is 1:0.5 to 1:
3.
7. A method for removing isocyanate impurities from an organic solvent, comprising the following steps: A mixed solution containing isocyanate, organic solvent and liquid phosgene in an isocyanate production system is subjected to a catalytic reaction by passing through a reactor loaded with the isocyanate polymerization catalyst according to claim 1. After the isocyanate is polymerized by the catalytic reaction, an isocyanate polymer is generated, which is then distilled and purified. The light component liquid phase at the top of the tower is used to obtain a purified organic solvent from which impurities are removed, and the heavy component liquid phase at the bottom of the tower is discharged and incinerated.
8. The method according to claim 7, characterized in that The catalytic reaction temperature is 10-50°C.
9. The method according to claim 7, characterized in that: The catalytic reaction temperature is 20-30°C.
Citation Information
Patent Citations
Imine-type quaternary ammonium salt catalyst, preparation method thereof and low-viscosity polyisocyanate composition prepared therefrom
CN109749036A
Equipment and process for recovering and purifying solvent o-dichlorobenzene in photochemical reaction process
CN110724029A
Application of aromatic hydrocarbon solvent in purification of p-phenylene diisocyanate and purification method
CN111825573A
Catalyst for hydrogenation of Fischer-Tropsch synthesis oil, preparation method as well as application thereof
CN101733119A
Catalyst for removing moisture in phosgene and method for removing moisture in phosgene in isocyanate production process
CN111715286A