A flexible conductive polymer material and its preparation method and application

By forming a dual crosslinking network structure in flexible conductive polymer materials, the problems of degradation of conductivity and lack of self-repair and recycling of existing materials under deformation are solved, and flexible conductive materials with high conductivity, high strength and environmental protection performance are achieved , suitable for smart wearable products.

CN116218112BActive Publication Date: 2024-11-19SUN YAT SEN UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310203011.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-03
Publication Date
2024-11-19
Estimated Expiration
2043-03-03

AI Technical Summary

Technical Problem

The conductivity of existing flexible conductive polymer materials decreases in stretching, bending and folding states, lacks self-repair and recycling performance, making it difficult to meet the high conductivity, high strength and environmental protection needs of smart wearable products.

Method used

The flexible polymer with reversible DA bond crosslinking and the conductive polymer with reversible imine bond crosslinking react with the linear polymer PEDOT:PSS to form a dual crosslinking network structure, through the 'forced mutual solubility' and 'mutual coordination' , build a multifunctional interlocking network to improve conductivity, strength and tolerance, and have self-healing and recyclable properties.

Benefits of technology

It achieves stable conductivity under deformation state, has high conductivity, high strength, self-repair and recyclable performance, and is suitable for smart wearable products, overcoming performance shortcomings and application limitations in the prior art.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116218112B_ABST
    Figure CN116218112B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of polymer materials, and specifically relates to a flexible conductive polymer material, a preparation method and an application thereof. The flexible conductive polymer material comprises the following components in parts by weight: 25 to 95 parts of a flexible polymer D containing reversible DA bond crosslinking; 0.025 to 40 parts of a conductive polymer S containing reversible imine bond crosslinking; 1 to 75 parts of a linear polymer PEDOT:PSS. The flexible conductive polymer material prepared by the present invention has the advantages of high conductivity, high strength, high tolerance, self-repairing and repeatable recycling, and has excellent comprehensive performance. It can overcome the shortcomings of the flexible conductive polymer materials in the prior art that cannot simultaneously have excellent conductivity, flexibility, stretchability, stable electrical and electrochemical properties in a deformed state, and economic and environmental protection characteristics.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polymer materials, and in particular relates to a flexible conductive polymer material and a preparation method and application thereof. Background Art

[0002] In the 21st century, with the rapid development of electronic information technology, smart wearable products have gradually entered various fields of human life, and have great application potential in health detection, sports assistance, human-computer interaction, etc. Flexible conductive materials are an indispensable component for the preparation of smart wearable products. Compared with inorganic and metal materials, conductive polymers have the characteristics of low cost, low density, easy processing, easy flexibility modification, and large-area film formation. Therefore, the use of conductive polymers as conductive matrix to prepare flexible conductive materials is more in line with practical application requirements such as softness, lightness, and low cost, and therefore has received more and more attention.

[0003] At present, according to different structures, flexible conductive polymer materials mainly have two forms: non-self-supporting and self-supporting. Non-self-supporting flexible conductive polymer materials have outstanding advantages: simple preparation, good conductivity in the plane direction, and early flexible conductive polymer materials are mainly non-self-supporting. However, the disadvantages of non-self-supporting flexible conductive polymers are also very obvious. For example, due to the brittleness of the conductive layer, the material has poor bending resistance and short service life; the conductivity is not good in the tensile state, and the conductivity decreases significantly under tension; it can only conduct electricity in the plane direction, but not in the cross-sectional direction; at the same time, non-self-supporting conductive polymer materials cannot self-repair and recycle. In practical applications, in order to match the performance requirements of wearable electronic devices, flexible conductive materials not only need to have excellent conductivity, but also have good flexibility, stretchability, and stable electrical and electrochemical properties under deformation. Based on environmental protection and economic considerations, ideal flexible conductive polymer materials also need to have self-repair and recyclability. Therefore, the above factors determine that the actual application scenarios of non-self-supporting flexible conductive polymer materials are very limited. Compared with non-self-supporting flexible conductive polymers, self-supporting flexible conductive polymers have a more stable structure and tighter connections because the conductive components are coated and evenly dispersed by the flexible components. Through reasonable design, it is expected to overcome all of the above disadvantages at the same time, so as to better meet the actual application needs and gain a wider application space.

[0004] It is worth pointing out that although there is a possibility of success for self-supporting conductive polymers, there are few reports on this technology that can overcome all the above disadvantages. The conductivity of most self-supporting flexible conductive polymer materials will drop significantly when stretched, bent, or folded, and they cannot work stably in flexible electronic devices in practical applications. At the same time, most self-supporting flexible conductive polymer materials do not have self-repairing and recycling properties, and cannot provide good environmental protection and economy. Therefore, it is urgent to construct a self-supporting flexible conductive polymer material with high conductivity, high strength, high tolerance, self-repairing and repeated recycling performance. Summary of the invention

[0005] The present invention aims to provide a flexible conductive polymer material and a preparation method and application thereof. The flexible conductive polymer material prepared by the present invention has the advantages of high conductivity, high strength and high tolerance, and has excellent comprehensive performance, and can overcome the shortcomings of the flexible conductive polymer material in the prior art that it cannot simultaneously have excellent conductivity, flexibility, stretchability, stable electrical and electrochemical properties in a deformed state, and economic and environmental protection characteristics.

[0006] In order to achieve the above object, the present invention adopts the following technical solution: a flexible conductive polymer material, comprising the following components in parts by weight:

[0007] 25 to 95 parts of a flexible polymer D containing reversible DA crosslinking;

[0008] 0.025 to 40 parts of a conductive polymer S containing reversible imine bond crosslinking;

[0009] Linear polymer PEDOT:PSS 1 to 75 parts.

[0010] Preferably, the flexible conductive polymer material comprises the following components in parts by weight:

[0011] 50 to 89.75 parts of a flexible polymer D containing reversible DA crosslinking;

[0012] 0.25 to 1.25 parts of a conductive polymer S containing reversible imine bond crosslinking;

[0013] Linear polymer PEDOT:PSS 10-48.75 parts;

[0014] The mass of the linear polymer PEDOT:PSS is 10-50% of the total mass of the flexible conductive polymer material.

[0015] In the present invention, the flexible polymer D containing reversible DA bond crosslinking, the conductive polymer S containing reversible imine bond crosslinking and the linear polymer PEDOT:PSS react with each other to form an interlocking network with a double crosslinking network structure, and multiple networks containing different functions are combined together by means of "forced mutual dissolution" and "mutual coordination", so that the obtained material obtains multifunctionality that is difficult to achieve with a single group of networks. The crosslinking structure of the formed interlocking network and the mutual restriction between the networks make the conductivity of the obtained flexible conductive polymer material have good deformation tolerance and very stable conductivity.

[0016] The present invention selects a flexible polymer D containing reversible DA bond crosslinking as a flexible component to provide flexibility to the composite material; and selects a combination of a conductive polymer S containing reversible imine bond crosslinking and a linear polymer PEDOT:PSS as a conductive component to provide good conductivity to the composite material. In addition to the performance of the single-group network itself possessed by the flexible polymer D containing reversible DA bond crosslinking and the conductive polymer S containing reversible imine bond crosslinking, due to the interlocking structure formed by the reaction, it also shows excellent network synergy, mainly due to the following aspects:

[0017] First, the three-dimensional conjugated cross-linked conductive polymer S containing reversible imine bonds can effectively construct a three-dimensional conductive path and increase the number of conductive paths, thereby improving the overall conductivity of the flexible conductive polymer material formed by the raw material components; at the same time, when the linear polymer PEDOT:PSS is added to the formula system, since the LUMO-HOMO energy level of the conductive polymer S containing reversible imine bonds is between the LUMO-LUMO energy levels of the linear polymer PEDOT:PSS, it can provide a transition state for the electronic transition of the linear polymer PEDOT:PSS, reduce the bandgap width of the transition of the linear polymer PEDOT:PSS, and further improve the conductive efficiency of the linear polymer PEDOT:PSS;

[0018] Second, the interlocking network structure formed has a stronger network restriction effect than a single group of networks, which can significantly improve the strength of the material;

[0019] Third, the interlocking network formed has better tolerance and can maintain good conductive stability under the action of solvents and mechanical deformation;

[0020] Fourth, since the flexible polymer D cross-linked by DA bonds and the conductive polymer S cross-linked by imine bonds are both dynamically reversible, the prepared flexible conductive polymer material has self-healing and recyclability.

[0021] In the present invention, the flexible polymer D containing reversible DA bond crosslinking and the conductive polymer S containing reversible imine bond crosslinking both contain only one reversible covalent bond that does not interfere with or react with each other. The flexible polymer D containing reversible DA bond crosslinking contains only one reversible covalent bond, namely DA bond, and does not contain other dynamic reversible bonds; the conductive polymer S containing reversible imine bond crosslinking contains only one reversible covalent bond, namely Schiff base bond, and does not contain other dynamic reversible bonds. The types and quantities of irreversible chemical bonds in the crosslinked polymers D and S are not limited.

[0022] The performance of the flexible conductive polymer material described in the present invention is most affected by the ratio of each component. Therefore, the present invention adjusts the performance of the interlocking network composite material by reasonably optimizing the ratio of each component, and finally obtains a series of flexible conductive polymer materials with different performance focuses.

[0023] Preferably, the polymer D containing reversible DA bond crosslinking comprises the following components in parts by weight:

[0024]

[0025] More preferably, the cross-linked polymer D containing reversible DA bonds comprises the following components in parts by weight:

[0026]

[0027] Preferably, the sulfonic acid group-containing monoolefin monomer comprises More preferably, the sulfonic acid group-containing monoolefin monomer is

[0028] Preferably, the monoalkenyl furan monomer comprises At least one of .

[0029] Preferably, the fluorine-containing monoolefin monomer comprises

[0030] At least one of .

[0031] More preferably, the fluorine-containing monoolefin monomer is At least one of .

[0032] Preferably, the polyethylene glycol monoolefin monomer comprises At least one of .

[0033] More preferably, the polyethylene glycol monoolefin monomer is The molecular weight is 300-1500.

[0034] Preferably, the acrylic acid ester monomers include More preferably, the acrylic acid ester monomer is

[0035] Preferably, the maleimide curing agent comprises At least one of .

[0036] More preferably, the maleimide curing agent is:

[0037] The method for preparing the polymer D containing reversible DA bond crosslinking comprises the following steps:

[0038] All monomers were added into the solvent, stirring and gas protection were started, the temperature was raised to the reaction temperature, initiator was added, and ventilation and stirring were continued. After the reaction was completed, the solvent was removed to obtain a yellow elastic solid. After washing, the solvent was removed to obtain a polymer D (light yellow elastomer) containing reversible DA bond crosslinking.

[0039] Wherein, the solvent is 2-acrylamide-2-methylpropanesulfonic acid aqueous solution (AMPS);

[0040] The reaction temperature is 60-80°C and the reaction time is 6-24h;

[0041] The initiator is azobisisobutyronitrile (AIBN);

[0042] The washing condition is to use ethanol as a solvent for 2 to 5 times;

[0043] The temperature of removing the solvent is 50-90°C.

[0044] Preferably, the conductive polymer S containing reversible imine bond crosslinking comprises the following components in parts by weight:

[0045] 64-95 parts of double-terminated amino-containing aniline oligomer;

[0046] 5 to 36 parts of polyaldehyde aromatic compounds.

[0047] More preferably, the conductive polymer S containing reversible imine bond crosslinking comprises the following components in parts by weight:

[0048] 90-95 parts of double-terminated amino-aniline oligomer;

[0049] 5 to 10 parts of polyaldehyde aromatic compounds.

[0050] Preferably, the chemical structural formula of the double-terminated amino-aniline oligomer is The degree of polymerization is 3 to 15. More preferably, the degree of polymerization of the double-terminated amino-group aniline oligomer is 8 to 14.

[0051] Preferably, the polyaldehyde aromatic compound includes at least one of trimesaldehyde and 3,4',5-trialdehyde-1,1-biphenyl. More preferably, the polyaldehyde aromatic compound is trimesaldehyde.

[0052] The method for preparing the conductive polymer S containing reversible imine bond crosslinking comprises the following steps:

[0053] Dissolving the double-terminated aminoaniline oligomer and the polyaldehyde aromatic compound in a solvent respectively, reacting them, and removing the solvent from the resulting solution to obtain the conductive polymer S containing reversible imine bond crosslinking;

[0054] The solvent is one of dimethyl sulfoxide and dimethylformamide or a combination of the two;

[0055] The reaction temperature is 10-100° C., and the reaction time is 2-48 hours.

[0056] Preferably, the double-terminated amino-group aniline oligomer comprises the following components in parts by weight:

[0057] 20-40 parts of aniline monomer;

[0058] 1 to 20 parts of molecular weight regulator;

[0059] 5-80 parts of oxidant;

[0060] More preferably, the double-terminated amino-group aniline oligomer comprises the following components in parts by weight:

[0061] 30.7 parts of aniline monomer;

[0062] 9.8 parts of molecular weight regulator;

[0063] 59.5 parts of oxidant.

[0064] Preferably, the molecular weight regulator is 4,4'-diaminodiphenylamine sulfate hydrate.

[0065] Preferably, the oxidant comprises one or more of ammonium persulfate, ferric chloride, and hydrogen peroxide. More preferably, the oxidant is ammonium persulfate.

[0066] Preferably, the method for preparing the double-terminated amino-group aniline oligomer comprises the following steps:

[0067] S1. Under the protection of inert gas, dissolve aniline monomer and molecular weight regulator in 2-acrylamide-2-methylpropanesulfonic acid aqueous solution (AMPS), stir and react;

[0068] S2, dissolving the oxidant in an aqueous solution of 2-acrylamide-2-methylpropanesulfonic acid, and then adding it to the solution of step S1, reacting, filtering, and washing the obtained precipitate to obtain a double-terminated amino-aniline oligomer.

[0069] More preferably, the method for preparing the double-terminated amino-group aniline oligomer comprises at least one of the following (1) to (5):

[0070] (1) The concentration of the 2-acrylamide-2-methylpropanesulfonic acid aqueous solution in steps S1 and S2 is 0.25 to 2 mol / L;

[0071] (2) the amount of the 2-acrylamide-2-methylpropanesulfonic acid aqueous solution added in step S1 is 20 to 40 times the total mass of the aniline monomer and the molecular weight regulator;

[0072] (3) the amount of the 2-acrylamide-2-methylpropanesulfonic acid aqueous solution added in step S2 is 5 to 10 times the mass of the oxidant;

[0073] (4) The washing conditions in step S2 are washing with water, ethanol, methanol, and ether in sequence until the filtrate is colorless;

[0074] (5) The reaction temperature in steps S1 and S2 is -10 to 30°C, and the reaction time is 2 to 48 hours.

[0075] The present invention also claims a method for preparing the flexible conductive polymer material, comprising the following steps:

[0076] The polymer D containing reversible DA bond crosslinking and the conductive polymer S containing reversible imine bond crosslinking are respectively thermally excited and dissolved in a solvent, and then the obtained solution is mixed with the linear polymer PEDOT:PSS for reaction, and the solvent is removed to obtain the flexible conductive polymer material.

[0077] Preferably, the preparation method comprises at least one of the following (1) to (5):

[0078] (1) The temperature of thermally stimulated dissolution of the polymer D containing reversible DA bond crosslinking is 90 to 140° C., and the dissolution time is 15 min to 8 h;

[0079] (2) The temperature of thermally excited dissolution of the conductive polymer S containing reversible imine bond crosslinking is 20 to 120° C., and the dissolution time is 30 min to 96 h;

[0080] (3) The solvent for thermally activating the dissolution of the polymer D containing reversible DA bond crosslinks is water; the solvent for thermally activating the dissolution of the conductive polymer S containing reversible imine bond crosslinks is dimethyl sulfoxide or dimethylformamide;

[0081] (4) The conditions for the mixed reaction of the solution and the linear polymer PEDOT:PSS are: reacting at 20 to 100° C. for 15 to 120 minutes;

[0082] (5) The process of removing the solvent is: evaporating at 70-90°C for 3-8 hours, and then continuing to evaporate at 60-80°C for more than 24 hours.

[0083] The electrical conductivity of the flexible conductive polymer material of the present invention can also be enhanced by at least one of annealing and solvent immersion.

[0084] Preferably, the annealing condition is annealing at 100-150° C. for 5-60 min, and the conductivity of the material is improved by high temperature annealing.

[0085] Preferably, the solution immersion is performed by immersing the material in one or more mixed solvents selected from the group consisting of dimethyl sulfoxide, ethylene glycol, water, dimethylformamide, methanol, ethanol, acetone, formamide, and glycerol to further improve the conductivity of the material.

[0086] The present invention also claims protection for the use of the flexible conductive polymer material in the preparation of conductive devices, luminescent materials, anti-corrosion materials, friction power generation materials, and sensor materials. The conductive devices include electrodes or circuits of electronic devices, battery or capacitor electrode materials, and the friction materials include friction generator friction materials, etc.

[0087] Compared with the prior art, the present invention has the following beneficial effects:

[0088] (1) It is difficult for the conductive polymer materials in the prior art to simultaneously achieve good results in tensile strength, elongation at break, conductivity and other properties (tensile strength greater than 10MPa, elongation at break greater than 50%, conductivity higher than 50S / cm). Generally, if the conductive performance is good, the tensile strength or elongation at break will be relatively low, or the elongation at break is high, but the tensile strength and conductivity are both low. The present invention can effectively overcome the problems existing in the prior art, and the obtained flexible conductive polymer material can simultaneously have the advantages of high conductivity, high strength and high tolerance, good self-repair and repeated recycling performance, etc., with excellent comprehensive performance, which is more in line with the actual application requirements.

[0089] (2) The resistance of the conductive polymer materials in the prior art will increase as the stretching progresses, while the flexible conductive polymer materials prepared by the present invention can almost keep the resistance unchanged before being broken, which has great significance for practical applications. BRIEF DESCRIPTION OF THE DRAWINGS

[0090] Figure 1 This is the FTIR spectrum of the flexible polymer D containing reversible DA bond crosslinking of the present invention.

[0091] Figure 2 This is the MALDI-TOF spectrum of the double-terminated amino-aniline oligomer (PANI) of the present invention.

[0092] Figure 3 This is the H-NMR spectrum of the conductive polymer S containing reversible imine bond cross-linking of the present invention.

[0093] Figure 4 This is a DSC diagram of an embodiment of the present invention.

[0094] Figure 5 It is a schematic diagram of the conductivity test of the present invention.

[0095] Figure 6 The resistance of Example 4 of the present invention changes with the immersion time in water.

[0096] Figure 7 The resistance variation trend of Example 4 of the present invention during the stretching process.

[0097] Figure 8 This is a schematic diagram of the self-repairing performance effect of Example 4 of the present invention.

[0098] Fig. 9 This is a schematic diagram of the heavy recovery performance effect of Example 4 of the present invention. DETAILED DESCRIPTION

[0099] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0100] In the embodiments and comparative examples, the experimental methods used are conventional methods unless otherwise specified, and the materials, reagents, etc. used are all commercially available unless otherwise specified.

[0101] The linear polymer PEDOT:PSS used in the examples and comparative examples of the present invention is a PEDOT:PSS solution (solid content calculated as 1.2%) with the manufacturer's brand: HeraeusClevios PH1000.

[0102] The flexible polymer D containing reversible DA bond crosslinking and the conductive polymer S containing reversible imine bond crosslinking selected in the examples of the present invention and comparative examples 1 to 3 are the same components and are prepared by the methods of examples 1 to 2.

[0103] Example 1, Preparation of Flexible Polymer D Containing Reversible DA Bond Crosslinking:

[0104] 2.72g of 2-acrylamide-2-methylpropanesulfonic acid aqueous solution (AMPS), 1.21g of polyethylene glycol methyl ether methacrylate, 7.93g of hexyl acrylate, 1.43g of 2,2,3,4,4,4-hexafluorobutyl acrylate and 0.23g of furfuryl methacrylate were dissolved in 40mL of dimethylformamide and added into a round-bottom three-necked flask with an argon protection device and a magnetic stirring device. After stirring and gas protection were turned on, the temperature was raised to 65°C. After reacting for 1h, 0.13g of initiator AIBN was added, and ventilation and stirring were continued for 12h, and then 0.23g of 4,4'-bismaleimidodiphenylmethane was added. After 1h, the solvent was removed from the reaction solution to obtain a yellow elastic solid. The crude product was stirred and washed 5 times with ethanol at room temperature, and the obtained solid product was dried at 60°C for 24h to obtain a flexible polymer D containing reversible DA bond crosslinking. The FTIR spectrum is shown in the attached figure. Figure 1 .

[0105] Example 2: Preparation of reversible imine bond cross-linked conductive polymer S:

[0106] a. Preparation of double-terminated amino-group aniline oligomer (PANI):

[0107] 1.39g aniline and 0.4675g 4,4'-diaminodiphenylamine sulfate hydrate were added to 50mL 0.5mol / L AMPS aqueous solution, added to a round-bottom three-necked flask with an argon protection device and mechanical stirring, and stirred under argon protection. The temperature dropped to 0°C. After 1 hour, 2.71g ammonium persulfate was dissolved in 20mL 0.5mol / L AMPS aqueous solution and added to the above system. After continuing the reaction for 10 hours, the filter cake was filtered and collected. The filter cake was washed with 0.05mol / L AMPS aqueous solution 5 times, methanol 3 times, ethanol 3 times, acetone 3 times, and anhydrous ether 2 times, and then vacuum dried at room temperature to obtain a black powder product PANI. The mass spectrum is shown in the attached Figure 2 ;

[0108] b. Preparation of reversible imine bond cross-linked conductive polymer S:

[0109] 1.0 g of PANI was added to 200 mL of dimethyl sulfoxide, added to a round-bottomed single-necked flask with a magnetic stirrer, and stirred at 30°C until dissolved. After dissolution, 0.13 g of trimesaldehyde was added and stirred at 40°C for 72 hours. Finally, the solvent was removed from the reaction solution to obtain a reversible imine bond cross-linked conductive polymer S. The H NMR spectrum is shown in the attached figure. Figure 3 .

[0110] Example 3: Flexible conductive polymer material and preparation method thereof

[0111] Raw materials: 94.875 parts of flexible polymer D containing reversible DA bond crosslinking;

[0112] 0.125 parts of a conductive polymer S containing reversible imine bond crosslinking;

[0113] Linear polymer PEDOT:PSS 5 parts.

[0114] Preparation method:

[0115] S1. Take the reversibly cross-linked flexible polymer D with DA bonds, add it to 190 mL of water, add it to a round-bottom three-necked flask equipped with a condenser, an argon protection device and a mechanical stirring device after it is fully swollen, and stir it at 100°C for 2 h to obtain a transparent solution;

[0116] S2. Take the conductive polymer S containing reversible imine bond crosslinking, add it to 2 mL of dimethyl sulfoxide, and after it is fully swollen, add it to a round-bottomed three-necked flask equipped with a condenser, an argon protection device and a mechanical stirring device, and stir at 80°C until it is completely dissolved;

[0117] S3. Take the linear polymer PEDOT:PSS, add the above two solutions to mix, and continue to stir at 70°C for 24 hours under argon protection, cast into a polytetrafluoroethylene mold, place it at 80°C for drying for 6 hours, and then continue to dry and cure at 70°C for more than 24 hours to finally obtain a flexible conductive polymer material, recorded as DS-5%.

[0118] Example 4: Flexible conductive polymer material and preparation method thereof

[0119] Raw materials: 89.75 parts of flexible polymer D containing reversible DA bond crosslinking;

[0120] 0.25 parts of a conductive polymer S containing reversible imine bond crosslinking;

[0121] Linear polymer PEDOT:PSS 10 parts.

[0122] Preparation method:

[0123] S1. Take the reversibly cross-linked flexible polymer D with DA bonds, add it to 190 mL of water, add it to a round-bottom three-necked flask equipped with a condenser, an argon protection device and a mechanical stirring device after it is fully swollen, and stir it at 100°C for 2 h to obtain a transparent solution;

[0124] S2. Take the conductive polymer S containing reversible imine bond crosslinking, add it to 2 mL of dimethyl sulfoxide, and after it is fully swollen, add it to a round-bottomed three-necked flask equipped with a condenser, an argon protection device and a mechanical stirring device, and stir at 80°C until it is completely dissolved;

[0125] S3. Take the linear polymer PEDOT:PSS, add the above two solutions to mix, and continue to stir at 70°C for 24 hours under argon protection, cast into a polytetrafluoroethylene mold, place it at 80°C for drying for 6 hours, and then continue to dry and cure at 70°C for more than 24 hours to finally obtain a flexible conductive polymer material, recorded as DS-10%.

[0126] Example 5: Flexible conductive polymer material (DS-1-10%) and preparation method thereof

[0127] Raw materials: 50 parts of flexible polymer D containing reversible DA bond crosslinking;

[0128] 40 parts of a conductive polymer S containing reversible imine bond crosslinking;

[0129] Linear polymer PEDOT:PSS 10 parts.

[0130] The preparation method is similar to that of Example 4.

[0131] Example 6: Flexible conductive polymer material (DS-2-10%) and preparation method thereof

[0132] Raw materials: 25 parts of flexible polymer D containing reversible DA bond crosslinking;

[0133] 0.025 parts of a conductive polymer S containing reversible imine bond crosslinking;

[0134] Linear polymer PEDOT:PSS 10 parts.

[0135] The preparation method is similar to that of Example 4.

[0136] Example 7, Flexible Conductive Polymer Material (DS-30%) and Preparation Method thereof Raw materials: 89.75 parts of flexible polymer D containing reversible DA bond crosslinking;

[0137] 0.25 parts of a conductive polymer S containing reversible imine bond crosslinking;

[0138] Linear polymer PEDOT:PSS 30 parts. Preparation method is as in Example 4.

[0139] Example 8, Flexible Conductive Polymer Material (DS-40%) and Preparation Method thereof Raw materials: 89.75 parts of flexible polymer D containing reversible DA bond crosslinking;

[0140] 0.25 parts of a conductive polymer S containing reversible imine bond crosslinking;

[0141] Linear polymer PEDOT:PSS 40 parts. Preparation method is as in Example 4.

[0142] Example 9, Flexible Conductive Polymer Material (DS-50%) and Preparation Method thereof Raw materials: 89.75 parts of flexible polymer D containing reversible DA bond crosslinking;

[0143] 0.25 parts of a conductive polymer S containing reversible imine bond crosslinking;

[0144] Linear polymer PEDOT:PSS 50 parts. Preparation method is as in Example 4.

[0145] Example 10, Flexible Conductive Polymer Material (DS-75%) and Preparation Method thereof Raw materials: 89.75 parts of flexible polymer D containing reversible DA bond crosslinking;

[0146] 0.25 parts of a conductive polymer S containing reversible imine bond crosslinking;

[0147] Linear polymer PEDOT:PSS 75 parts. Preparation method is as in Example 4.

[0148] Comparative Example 1

[0149] Raw materials: 100 parts of flexible polymer D containing reversible DA bond cross-linking;

[0150] 0.01 part of a conductive polymer S containing reversible imine bond crosslinking;

[0151] Linear polymer PEDOT:PSS 10 parts. Preparation method is as in Example 4.

[0152] Comparative Example 2

[0153] Raw materials: 90 parts of flexible polymer D containing reversible DA bond crosslinking;

[0154] Linear polymer PEDOT:PSS 10 parts.

[0155] Preparation method:

[0156] S1. Take the reversibly cross-linked flexible polymer D with DA bonds, add it to 190 mL of water, add it to a round-bottom three-necked flask equipped with a condenser, an argon protection device and a mechanical stirring device after it is fully swollen, and stir it at 100°C for 2 h to obtain a transparent solution;

[0157] S2. Take a linear polymer PEDOT:PSS, add it to the above solution and mix it. Continue stirring at 70°C for 24 hours under argon protection, cast it into a polytetrafluoroethylene mold, dry it at 80°C for 6 hours, and then continue drying and curing at 70°C for more than 24 hours to finally obtain a flexible conductive polymer material, recorded as D-10%.

[0158] The only difference between this comparative example and Example 4 is that the conductive polymer S containing reversible imine bond crosslinking is replaced by an equal amount of the flexible polymer D containing reversible DA bond crosslinking.

[0159] Comparative Example 3

[0160] Compared with Example 4, the only difference of this comparative example is that the linear polymer PEDOT:PSS is not added.

[0161] The preparation method is similar to that of Example 4.

[0162] Comparative Example 4

[0163] This comparative example provides a non-interlocking, non-crosslinked comparative sample, which is a conductive polymer obtained by directly blending linear polymers.

[0164] Preparation method: 0.53g AMPS, 0.24g polyethylene glycol methyl ether methacrylate, 1.58g hexyl acrylate, 0.28g 2,2,3,4,4,4-hexafluorobutyl acrylate and 0.04g furfuryl methacrylate were dissolved in 10mL dimethylformamide, added to a round-bottomed three-necked flask with an argon protection device and a magnetic stirring device, and the temperature was raised to 65°C after stirring and gas protection. After 1h, 0.04g initiator AIBN was added, and ventilation and stirring were continued for 12h. After the reaction was completed, the above solution was mixed with 25.41g linear polymer PEDOT:PSS, and continued to stir at 70°C for 24h under argon protection, cast into a polytetrafluoroethylene mold, placed at 80°C for 6h, and then placed at 70°C for more than 24h to finally obtain a black elastic film product, recorded as LM-10%.

[0165] Comparative Example 5

[0166] Preparation of flexible polymer D-1 containing reversible DA bond crosslinking:

[0167] 2.72 g of 2-acrylamide-2-methylpropanesulfonic acid aqueous solution (AMPS), 1.21 g of polyethylene glycol methyl ether methacrylate, 7.93 g of hexyl acrylate, 1.43 g of n-butyl acrylate and 0.23 g of furfuryl methacrylate were dissolved in 40 mL of dimethylformamide and added into a round-bottom three-necked flask with an argon protection device and a magnetic stirring device. After stirring and gas protection were turned on, the temperature was raised to 65°C. After reacting for 1 hour, 0.13 g of initiator AIBN was added, and ventilation and stirring were continued for 12 hours. Then, 0.23 g of 4,4'-bismaleimidodiphenylmethane was added. After 1 hour, the solvent was removed from the reaction solution to obtain a yellow elastic solid. The crude product was stirred and washed 5 times with ethanol at room temperature. The obtained solid product was dried at 60°C for 24 hours to obtain a flexible polymer D-1 containing reversible DA bond crosslinks.

[0168] The preparation method of the conductive polymer S containing reversible imine bond crosslinking is the same as that in Example 2.

[0169] Raw materials for flexible conductive polymer materials:

[0170] 89.75 parts of a flexible polymer D-1 containing reversible DA crosslinking;

[0171] 0.25 parts of a conductive polymer S containing reversible imine bond crosslinking;

[0172] Linear polymer PEDOT:PSS 10 parts.

[0173] The preparation method of the flexible conductive polymer material is referred to Example 4.

[0174] Compared with Example 4, the only difference of this comparative example is that an equal amount of n-butyl acrylate is used to replace 2,2,3,4,4,4-hexafluorobutyl acrylate (fluorinated monoolefin monomer).

[0175] Comparative Example 6

[0176] The preparation method of the flexible polymer D containing reversible DA bond crosslinking is the same as that of Example 1;

[0177] Preparation method of conductive polymer S-1 containing reversible imine bond cross-linking:

[0178] a. Preparation of double-terminated amino-group aniline oligomer (PANI):

[0179] 1.39g aniline and 0.4675g p-phenylenediamine were added to 50mL 0.5mol / L AMPS aqueous solution, and added to a round-bottom three-necked flask with an argon protection device and mechanical stirring. Under argon protection, stirring was started, and the temperature was reduced to 0°C. After 1 hour, 2.71g ammonium persulfate was dissolved in 20mL 0.5mol / L AMPS aqueous solution and added to the above system. After continuing the reaction for 10 hours, the filter cake was filtered and collected. The filter cake was washed with 0.05mol / L AMPS aqueous solution 5 times, methanol 3 times, ethanol 3 times, acetone 3 times, and anhydrous ether 2 times, and then vacuum dried at room temperature to obtain a black powder product PANI;

[0180] b. Preparation of reversible imine bond cross-linked conductive polymer S-1:

[0181] 1.0 g of PANI was added to 200 mL of dimethyl sulfoxide, added to a round-bottom single-necked flask with a magnetic stirrer, and stirred at 30°C until dissolved. After dissolution, 0.13 g of trimesaldehyde was added, and stirred at 40°C for 72 hours. Finally, the solvent was removed from the reaction solution to obtain a reversible imine bond cross-linked conductive polymer S-1.

[0182] Raw materials for flexible conductive polymer materials:

[0183] 89.75 parts of a flexible polymer D containing reversible DA crosslinking;

[0184] 0.25 parts of a conductive polymer S-1 containing reversible imine bond crosslinking;

[0185] Linear polymer PEDOT:PSS 10 parts.

[0186] The preparation method of the flexible conductive polymer material is referred to Example 4.

[0187] Compared with Example 4, the only difference of this comparative example is that p-phenylenediamine is used to replace 4,4'-diaminodiphenylamine sulfate hydrate (molecular weight regulator).

[0188] Test Example 1: Tensile and Conductive Performance Test

[0189] The performance of the flexible conductive polymer materials prepared in Examples 3 to 10 and Comparative Examples 1 to 6 was tested, and the test items were as follows:

[0190] (1) Tensile performance test:

[0191] The obtained material was cut into dumbbell-shaped test specimens with a width of 2 mm, and its stress-strain curve was recorded at a tensile rate of 5 mm / min. The test temperature was room temperature. The tensile strength results of the flexible conductive polymer material are shown in Table 1, and the elongation at break data of Examples 3 to 10 are shown in Table 2.

[0192] (2) Conductivity test:

[0193] After the obtained material was soaked in dimethyl sulfoxide for 12 hours, it was cut into strips with a length and width of 2cm×0.5cm, and silver was coated on both ends as electrodes. According to the formula: Test its conductivity. The test diagram is as attached. Figure 5 As shown in the attached Figures 6-7 The results are shown in Table 1.

[0194] Table 1 Tensile strength and conductivity data of each group

[0195]

[0196]

[0197] Table 2 Elongation at break of the embodiments of the present invention

[0198] Test items Elongation at break (%) Example 3 411.96 Example 4 177.97 Example 5 50.61 Example 6 84.97 Example 7 92.60 Example 8 83.29 Example 9 77.42 Example 10 52.01

[0199] From the data in Tables 1 to 2, it can be seen that the flexible polymer material prepared by the present invention can simultaneously have good electrical conductivity, flexibility, stretchability and other properties. The flexible polymer materials prepared in Examples 4 to 10 can simultaneously meet the requirements of tensile strength greater than 10 MPa, elongation at break greater than 50%, and electrical conductivity greater than 50 S / cm. The reason why the electrical conductivity of Example 3 is lower than 50 S / cm is that the proportion of the conductive polymer S containing reversible imine bond crosslinking and the linear polymer PEDOT:PSS in the formula system is relatively low, resulting in a lower final electrical conductivity.

[0200] From the attached Figure 4 It can be seen that the flexible conductive polymer materials prepared in Examples 3 to 10 of the present invention all have only one glass transition, indicating that the components are evenly distributed and no obvious phase separation occurs. Figures 6-7 It can be seen that due to the excellent network confinement effect of the interlocking network in the flexible conductive polymer material prepared in Example 4 of the present invention, the interlocking network structure is very stable and can well maintain the stability of conductivity under solvent immersion and tensile deformation.

[0201] The weight proportions of the flexible polymer D containing reversible DA bond crosslinking and the conductive polymer S containing reversible imine bond crosslinking added in Comparative Example 1 are not appropriate, and the tensile strength, elongation at break and other properties of the obtained flexible conductive polymer material are inferior to those of Example 4;

[0202] The material prepared in Comparative Example 2 does not have an interlocking structure. Although it contains the same amount of linear polymer PEDOT:PSS as Example 4, the conductivity of Comparative Example 2 without adding the conductive polymer S containing reversible imine bonds cross-linking is only 47.8% of that of the interlocking network Example 4, and the tensile strength of Comparative Example 2 is also lower than that of Example 4, indicating that the conductive polymer S containing reversible imine bonds cross-linking can effectively improve the conductive efficiency of the flexible conductive polymer material, and the interlocking structure is conducive to the improvement of strength;

[0203] In Comparative Example 3, no linear polymer PEDOT:PSS was added, and the conductive properties of the obtained material were significantly worse than those of the embodiment;

[0204] The flexible conductive polymer material prepared in Comparative Example 4 is a non-interlocking, linear blended structure. According to the performance comparison, it can be seen that the tensile strength and conductivity of the linear blended comparison sample without an interlocking structure are much lower than the interlocking network of Example 4, indicating that the interlocking structure of the present invention has significant advantages in performance;

[0205] In Comparative Examples 5 to 6, due to inappropriate raw material components added, the flexibility, conductivity and other properties of the prepared materials are inferior to those of the embodiments.

[0206] Test Example 2: Self-repair and recyclability test

[0207] 1. Self-repair performance test:

[0208] The material prepared in Example 4 was cut into strips with a length and width of 2 cm×0.5 cm. Scratches were introduced on the surface of the material using a sharp blade. After heat treatment (150°C-1h), the scratch repair was observed using an ultra-depth of field three-dimensional microscope. The results are shown in Figure 8 .

[0209] 2. Recyclability test:

[0210] The film material prepared in Example 4 was cut into pieces and subjected to heat pressing (150°C, 30 min, 30 MPa) to observe whether the material could be re-filmed. The results are shown in FIG. Fig. 9 .

[0211] From the attached Figures 8-9 It can be seen that the flexible conductive polymer material prepared in Example 4 of the present invention has good self-repair and recycling properties. This is because the two groups of networks that constitute the interlocking network are cross-linked by dynamic reversible bonds. Therefore, the interlocking network can be self-repaired and recycled by thermal excitation.

[0212] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical concept disclosed by the present invention shall still be covered by the claims of the present invention.

Claims

1. A flexible conductive polymer material, characterized in that: The composition comprises the following components in parts by weight: 25 to 95 parts of a flexible polymer D containing reversible DA crosslinking; 0.025 to 40 parts of a conductive polymer S containing reversible imine bond crosslinking; Linear polymer PEDOT:PSS 1-75 parts; The raw materials of the reversibly cross-linked polymer D include the following components in parts by weight: The weight portion of the fluorine-containing monoolefin monomer is not 0; The raw material of the conductive polymer S containing reversible imine bond crosslinking comprises the following components in parts by weight: 64-95 parts of double-terminated amino-containing aniline oligomer; 5 to 36 parts of polyaldehyde aromatic compounds; The raw materials of the double-terminated amino-aniline oligomer include the following components in parts by weight: 20-40 parts of aniline monomer; 1 to 20 parts of molecular weight regulator; 5-80 parts of oxidant; The molecular weight regulator is 4,4'-diaminodiphenylamine sulfate hydrate.

2. The flexible conductive polymer material according to claim 1, characterized in that: The composition comprises the following components in parts by weight: 50 to 89.75 parts of a flexible polymer D containing reversible DA crosslinking; 0.25 to 1.25 parts of a conductive polymer S containing reversible imine bond crosslinking; Linear polymer PEDOT:PSS 10-48.75 parts; The mass of the linear polymer PEDOT:PSS is 10-50% of the total mass of the flexible conductive polymer material.

3. The flexible conductive polymer material according to claim 1, characterized in that: The method for preparing the conductive polymer S containing reversible imine bond crosslinking comprises the following steps: Dissolving the double-terminated aminoaniline oligomer and the polyaldehyde aromatic compound in a solvent respectively, reacting them, removing the solvent from the resulting solution, and obtaining the conductive polymer S containing reversible imine bond crosslinking; The solvent is one of dimethyl sulfoxide and dimethylformamide or a combination of the two; The reaction temperature is 10-100° C., and the reaction time is 2-48 hours.

4. The flexible conductive polymer material according to claim 1, characterized in that: The conductivity of the flexible conductive polymer material is enhanced by at least one of annealing and solvent immersion.

5. A method for preparing a flexible conductive polymer material as claimed in any one of claims 1 to 4, characterized in that: The following steps are involved: The polymer D containing reversible DA bond crosslinking and the conductive polymer S containing reversible imine bond crosslinking are respectively thermally excited and dissolved in a solvent, and then the obtained solution is mixed with the linear polymer PEDOT:PSS for reaction, and the solvent is removed to obtain the flexible conductive polymer material.

6. The preparation method according to claim 5, characterized in that: At least one of the following (1) to (5): (1) The temperature of thermally stimulated dissolution of the polymer D containing reversible DA bond crosslinking is 90 to 140° C., and the dissolution time is 15 min to 8 h; (2) The temperature of thermally excited dissolution of the conductive polymer S containing reversible imine bond crosslinking is 20 to 120° C., and the dissolution time is 30 min to 96 h; (3) The solvent for thermally activating the dissolution of the polymer D containing reversible DA bond crosslinks is water; the solvent for thermally activating the dissolution of the conductive polymer S containing reversible imine bond crosslinks is dimethyl sulfoxide or dimethylformamide; (4) The conditions for the mixed reaction of the solution and the linear polymer PEDOT:PSS are: reacting at 20 to 100° C. for 15 to 120 minutes; (5) The process of removing the solvent is: evaporating at 70-90°C for 3-8 hours, and then continuing to evaporate at 60-80°C for more than 24 hours.

7. Use of the flexible conductive polymer material as claimed in any one of claims 1 to 4 in the preparation of conductive devices, luminescent materials, anti-corrosion materials, friction power generation materials, and sensor materials.