A method for preparing a high damage-resistant particle-reinforced aluminum-based composite material plate
The preparation method of ceramic particle-reinforced aluminum-based composite materials uses homogenization treatment, rough rolling, solid solution and thermal-electrical coupling rolling processes to solve the deficiencies in high strength and fatigue properties of aluminum alloy materials and achieve high strength. and excellent fatigue properties, reducing heat treatment steps.
Patent Information
- Application Number
- CN202310171904.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-23
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2043-02-23
AI Technical Summary
Existing aluminum alloy materials are difficult to meet the requirements of high modulus, high strength and fatigue performance in the aerospace and automotive fields, and the traditional rolling process results in low plate strength, reduced elongation and poor fatigue performance.
The preparation method of ceramic particle-reinforced aluminum matrix composite materials is adopted, including homogenization treatment, preliminary rolling, solid solution treatment and thermal-electrical coupling rolling. Nano-scale short-range ordered structures are dynamically precipitated through a multi-field coupling process and evenly distributed in the matrix. , improve strength and fatigue properties.
The strength and fatigue properties of aluminum-based composite plates are improved, the fatigue crack growth rate is reduced, and the subsequent heat treatment process is reduced.
Smart Images

Figure CN116219334B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of metal material processing, and in particular to a method for preparing a high damage-resistant particle-reinforced aluminum-based composite material plate. Background Art
[0002] Aluminum alloy is widely used in the aerospace field due to its medium strength, good plasticity, good corrosion resistance and excellent damage tolerance. However, with the development of the aerospace and automotive fields, alloy materials are difficult to meet the requirements of high modulus, high strength and fatigue performance. Particle-reinforced metal matrix composites have received more attention and extremely broad application prospects in the fields of aerospace and automobiles due to their high specific strength, high specific modulus, excellent wear resistance and fatigue performance.
[0003] Compared with other traditional metal-based composite materials, in-situ self-generated nano-ceramic particle reinforced aluminum-based composite materials have better comprehensive mechanical properties and have great application potential in the field of structural materials. Since in-situ self-generated nano-ceramic particle reinforced aluminum-based composite materials have good plasticity, aluminum-based composite thin plates can be prepared by rolling process. However, the rolled plates usually have coarse grains and sufficient recrystallization, resulting in low strength of the plates. In addition, for heat-treatable alloy matrices, a large amount of precipitated phases precipitate after conventional artificial aging (peak aging), which improves the strength to a certain extent, but will lead to a decrease in elongation, which is not conducive to fatigue performance. Summary of the invention
[0004] To solve the above problems, the present invention provides a method for preparing a highly damage-resistant particle-reinforced aluminum-based composite material plate, comprising the following steps: (1) homogenizing a ceramic particle-reinforced aluminum-based composite material ingot; (2) initially rolling the ceramic particle-reinforced aluminum-based composite material ingot into a plate blank; (3) performing a solid solution treatment on the plate blank; and (4) performing a thermal-electric coupled rolling on the plate blank to obtain a particle-reinforced aluminum-based composite material plate.
[0005] Furthermore, the ceramic particle reinforced aluminum-based composite material is a 3.5wt.% TiB2 / 7050 aluminum-based composite material.
[0006] Furthermore, the ceramic particle reinforced aluminum-based composite material is a 5wt.% TiB2 / 2026 aluminum-based composite material.
[0007] Furthermore, the ceramic particle reinforced aluminum matrix composite material is 8wt.% TiB2 / 6061.
[0008] Furthermore, the thickness of the plate blank obtained by initial rolling is in the range of 4-20 mm.
[0009] Furthermore, during the solution treatment, the solution temperature is 480°C, the holding time is 1.5h, and then it is quickly cooled in cold water with a water temperature of less than 20°C.
[0010] Furthermore, during the thermo-electric coupling rolling, the roller temperature is 80°C, the pulse current is 500A, and the frequency is 100Hz; multiple passes and reciprocating rolling are performed, the pressing amount of a single pass is 2%, and the final rolling thickness is 8mm; water cooling is performed before each rolling pass to keep the plate temperature below 50°C.
[0011] Furthermore, after the plate is rolled to a target thickness, the plate is cooled in water and then kept warm in an environment with an air temperature of 60° C. for 1 day.
[0012] Furthermore, the positive and negative electrodes of the pulse power supply are connected to the upper roller and the lower roller respectively through a pair of springs and a conductive ball head; the conductive ball head contacts the rolling surfaces of the upper and lower rollers under the action of the spring. When the sheet blank is subjected to thermal-electric coupling rolling, the pulse power supply applies a pulse current to the upper and lower rollers and the sheet blank through the conductive ball head.
[0013] The present invention provides a multi-field coupled rolling process, which allows the aluminum-based composite material plate to dynamically precipitate a nanometer-scale short-range ordered structure during the rolling process and evenly distribute it in the matrix, thereby improving the strength and fatigue performance of the plate. The present invention achieves grain structure, precipitation phase and dislocation density control during the rolling process through the coupling of thermal field and electric field, obtains a uniformly dispersed nanometer short-range ordered structure and strengthening phase in the matrix, thereby improving the strength of the particle-reinforced aluminum-based composite material plate while improving plasticity and reducing the fatigue crack growth rate. At the same time, the subsequent heat treatment process can be reduced.
[0014] The concept, specific structure and technical effects of the present invention will be further described below in conjunction with the accompanying drawings to fully understand the purpose, characteristics and effects of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] Figure 1 The present invention is a flow chart of a method for preparing a highly damage-resistant particle-reinforced aluminum-based composite material plate.
[0016] Figure 2 Schematic diagram of thermal-electrical coupled rolling of plate billet. DETAILED DESCRIPTION
[0017] The following describes several preferred embodiments of the present invention with reference to the drawings in the specification, so that the technical content is clearer and easier to understand. The present invention can be embodied in many different forms of embodiments, and the protection scope of the present invention is not limited to the embodiments mentioned in the text.
[0018] like Figure 1As shown, the preparation method of the high damage-resistant particle-reinforced aluminum-based composite material plate of the present invention mainly includes the following steps:
[0019] (1) homogenizing the ceramic particle reinforced aluminum matrix composite ingot;
[0020] (2) initially rolling the ceramic particle reinforced aluminum matrix composite ingot into a plate blank;
[0021] (3) performing solution treatment on the sheet blank;
[0022] (4) The plate blank is subjected to thermal-electric coupled rolling to obtain a particle-reinforced aluminum-based composite plate.
[0023] like Figure 2 As shown, the positive and negative electrodes of the pulse power supply 4 are connected to the upper roller 1 and the lower roller 2 respectively through the spring 5 and the conductive ball head 6. The conductive ball head 6 contacts the rolling surface of the roller under the action of the spring 5. When the sheet blank 3 is thermo-electrically coupled rolled, the pulse power supply 4 applies a pulse current to the upper and lower rollers and the sheet blank 3 through the conductive ball head 6. Compared with the pulse power supply directly connecting the positive and negative electrodes to the rollers, this method of applying the pulse current does not require electrical modification of the rollers themselves, and can be directly used for ordinary rollers. It has a wider range of applications and is more flexible to use.
[0024] Example 1
[0025] Firstly, a 3.5wt.% TiB2 / 7050 aluminum-based composite ingot is homogenized at a homogenization temperature of 475°C for a holding time of 12-24h, followed by air cooling.
[0026] Secondly, the 3.5wt.% TiB2 / 7050 aluminum-based composite material ingot was rolled at 420°C to a size of 16 mm.
[0027] Then, a solution treatment was carried out at a solution temperature of 480°C and a holding time of 1.5 h, followed by rapid cooling in cold water at a water temperature of ~20°C.
[0028] The quenched plate is quickly transferred to the rolling mill for thermal-electric coupling rolling. The roller temperature is 80°C, the pulse current is 500A, and the frequency is 100Hz. Multiple passes are performed, and reciprocating rolling is performed with a small deformation amount. The pressing amount of a single pass is 2%, and the final rolling thickness is 8mm. Water cooling is performed before each rolling pass, and the plate temperature must be below 50°C.
[0029] Finally, the board was cooled in water and then kept warm for 1 day in an air temperature environment of 60°C.
[0030] Mechanical properties tests show that the final 3.5wt.% TiB2 / 7050 aluminum matrix composite material has a yield strength of 560MPa, a tensile strength of 620MPa, and an elongation of 12%. When the stress intensity factor range is ΔK = 15MPa·m 0.5 When the fatigue crack growth rate is 3×10 -4 mm / cycle.
[0031] Example 2
[0032] Firstly, a 5wt.% TiB2 / 2026 aluminum-based composite ingot was homogenized at a homogenization temperature of 495°C for a holding time of 36 hours, followed by air cooling.
[0033] Secondly, the 5wt.% TiB2 / 2026 aluminum-based composite ingot was rolled at 450°C to a length of 6 mm.
[0034] Then, a solution treatment was carried out at a solution temperature of 510°C and a holding time of 1 h, followed by rapid cooling in cold water at a water temperature of ~20°C.
[0035] The quenched plate is quickly transferred to the rolling mill for thermal-electric coupling rolling. The roller temperature is 80°C, the pulse current is 100A, and the frequency is 1000Hz. Multiple passes are performed, and reciprocating rolling is performed with a small deformation amount. The pressing amount of a single pass is 1%, and the final rolling thickness is 2mm. Water cooling is performed before each rolling pass, and the plate temperature must be below 50°C.
[0036] Finally, the board was cooled in water and then placed naturally in the air for 4 days.
[0037] Mechanical properties tests show that the final 5wt.% TiB2 / 2026 aluminum matrix composite material has a yield strength of 480MPa, a tensile strength of 590MPa, and an elongation of 16%. When the stress intensity factor range is ΔK = 15MPa·m 0.5 When the fatigue crack growth rate is 1×10 -4 mm / cycle.
[0038] Example 3
[0039] Firstly, the 8wt.% TiB2 / 6061 aluminum-based composite ingot was homogenized at a temperature of 550°C for 48 hours, followed by air cooling.
[0040] Secondly, the 8wt.% TiB2 / 6061 aluminum-based composite ingot was rolled at 460°C to a length of 20 mm.
[0041] Then, a solution treatment was carried out at a solution temperature of 565°C and a holding time of 2 h, followed by rapid cooling in cold water at a water temperature of ~20°C.
[0042] The quenched plate is quickly transferred to the rolling mill for thermal-electric coupling rolling. The roller temperature is 80°C, the pulse current is 300A, and the frequency is 500Hz. Multiple passes are performed, and reciprocating rolling is performed with a small deformation amount. The pressing amount of a single pass is 1%, and the final rolling thickness is 10mm. Water cooling is performed before each rolling pass, and the plate temperature must be below 50°C.
[0043] Finally, the plate was cooled in water and then kept warm for 1 day in an air temperature of 80°C. 0.5 When the fatigue crack growth rate is 5×10 -4 mm / cycle.
[0044] Mechanical property tests show that the final 8wt.% TiB2 / 6061 aluminum-based composite material has a yield strength of 270 MPa, a tensile strength of 310 MPa, and an elongation of 10%.
[0045] Comparative Example 1
[0046] The 3.5wt.% TiB2 / 7050 aluminum matrix composite material was rolled using a conventional rolling process. First, the ingot was homogenized at 465°C for 24 hours and then air-cooled.
[0047] The homogenized 3wt.% TiB2 / 7050 aluminum-based composite material was rolled at 460°C to a thickness of 8 mm.
[0048] Then the solution treatment is carried out with a solution temperature of 480°C and a holding time of 1.5h, followed by rapid cooling in cold water with a water temperature of ~20°C. Finally, the plate is aged at 120°C for 24h to reach peak aging.
[0049] Mechanical properties tests show that the final 3.5wt.% TiB2 / 7050 aluminum matrix composite material has a yield strength of 450MPa, a tensile strength of 560MPa, and an elongation of 11%. When the stress intensity factor range is ΔK = 15MPa·m 0.5 When the fatigue crack growth rate is 8×10 -4 mm / cycle.
[0050] Comparative Example 2
[0051] The 5wt.% TiB2 / 2026 aluminum-based composite material was rolled using a conventional rolling process. First, the 5wt.% TiB2 / 2026 aluminum-based composite material ingot was homogenized at 490°C for 48 hours and then air-cooled.
[0052] The homogenized 5wt.% TiB2 / 2026 aluminum-based composite material was rolled at 420°C to a thickness of 6 mm, and then cold-rolled to a thickness of 2 mm.
[0053] Then the steel was subjected to solution treatment at a temperature of 510°C and a holding time of 1 h, followed by rapid cooling in cold water at a water temperature of ~20°C, and finally subjected to natural failure for 4 days.
[0054] Mechanical properties tests show that the final 5wt.% TiB2 / 2026 aluminum matrix composite material has a yield strength of 320MPa, a tensile strength of 500MPa, and an elongation of 15%. When the stress intensity factor range is ΔK = 15MPa·m 0.5 When the fatigue crack growth rate is 5×10 -4 mm / cycle.
[0055] Comparative Example 3
[0056] The 8wt.% TiB2 / 6061 aluminum-based composite material was rolled using a conventional rolling process. First, the 8wt.% TiB2 / 6061 aluminum-based composite material ingot was homogenized at 550°C for 48 hours and then air-cooled.
[0057] The homogenized 5wt.% TiB2 / 2026 aluminum-based composite material was rolled at 4620°C to a thickness of 10 mm.
[0058] Then the steel was solution treated at 565°C for 2 h, followed by rapid water quenching, and finally aged at 180°C for 20 h to achieve peak aging.
[0059] Mechanical properties tests show that the final 8wt.% TiB2 / 6061 aluminum matrix composite material has a yield strength of 230MPa, a tensile strength of 290MPa, and an elongation of 10%. When the stress intensity factor range is ΔK = 15MPa·m 0.5 When the fatigue crack growth rate is 1×10 -3 mm / cycle.
[0060] From Examples 1-3 and Comparative Examples 1-3, it can be seen that the mechanical properties of the ceramic particle reinforced aluminum-based composite material subjected to the heat treatment process of the present invention are improved and the fatigue crack growth rate is reduced.
[0061] The preferred specific embodiments of the present invention are described in detail above. It should be understood that ordinary technicians in the field can make many modifications and changes based on the concept of the present invention without creative work. Therefore, all technical solutions that can be obtained by technicians in the technical field based on the concept of the present invention through logical analysis, reasoning or limited experiments on the basis of the prior art should be within the scope of protection determined by the claims.
Claims
1. A method for preparing a ceramic particle reinforced aluminum-based composite material plate, It is characterized in that Includes steps: (1) Homogenizing the ceramic particle reinforced aluminum matrix composite ingot; (2) rolling the ceramic particle reinforced aluminum matrix composite ingot into a plate blank; (3) Solution treatment of the sheet blank; (4) The plate blank is subjected to thermo-electric coupling rolling to obtain a particle-reinforced aluminum-based composite material plate; the positive and negative electrodes of the pulse power supply are connected to the upper roller and the lower roller respectively through a pair of springs and a conductive ball head; the conductive ball head contacts the rolling surface of the upper and lower rollers under the action of the spring; when the plate blank is subjected to thermo-electric coupling rolling, the pulse power supply applies a pulse current to the upper and lower rollers and the plate blank through the conductive ball head. During thermo-electric coupling rolling, the roller temperature is 80°C, the pulse current is 500 A, and the frequency is 100 Hz; multiple passes are performed, and reciprocating rolling is performed, with a single pass pressing amount of 2%, and finally rolled to a thickness of 8 mm; water cooling is performed before each rolling pass to keep the plate temperature below 50°C.
2. The method for preparing the ceramic particle reinforced aluminum-based composite material plate according to claim 1, in, Ceramic particle reinforced aluminum matrix composite material is 3.5wt.%TiB 2 / 7050 aluminum matrix composite material.
3. The method for preparing the ceramic particle reinforced aluminum matrix composite material plate according to claim 1, in, Ceramic particle reinforced aluminum matrix composite material is 5wt.%TiB 2 / 2026 aluminum matrix composite material.
4. The method for preparing the ceramic particle reinforced aluminum matrix composite material plate according to claim 1, in, Ceramic particle reinforced aluminum matrix composite material is 8wt.%TiB 2 / 6061.
5. The method for preparing the ceramic particle reinforced aluminum matrix composite material plate according to claim 1, in, During the solution treatment, the solution temperature is 480°C, the holding time is 1.5 h, and then it is quickly cooled in cold water with a water temperature of less than 20°C.
6. The method for preparing the ceramic particle reinforced aluminum matrix composite material plate according to claim 1, in, After the plate was rolled to the target thickness, it was cooled in water and then kept in an air temperature environment of 60°C for 1 day.