Polyimide nanofiber flakes and preparation method thereof

By preparing polyimide nanofiber floss in a conventional environment, using hot melt and partially molten polyamic acid spinning liquid to form a composite nanofiber film, and undergoing thermal imidation treatment, the floss in the prior art is solved The problem of unstable structure of the sheet and poor warmth preservation achieves efficient wind protection and warmth preservation.

CN116219629BActive Publication Date: 2024-11-12JIANGXI ADVANCED NANOFIBER S&T CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310398397.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-14
Publication Date
2024-11-12
Estimated Expiration
2043-04-14

AI Technical Summary

Technical Problem

The existing polyimide nanofiber flosses have decreased warmth when there is wind or temperature difference is large, and the preparation process depends on a high humidity environment, resulting in structural instability and poor compression, making it difficult to meet the application requirements of warmth materials.

Method used

The hot melt and partially molten polyamic acid spinning liquid were synthesized using diamine and dianhydride monomers to form a composite nanofiber membrane by electrospinning, and then the thermal imidation was carried out after the insulating fiber web was loosened to form a Multi-layer structure polyimide nanofiber floss.

Benefits of technology

It has achieved large-scale production of polyimide nanofiber floss in conventional environments, which has excellent wind resistance, warmth, compressibility and resilience, avoids flying floss, and improves the long-term useability and warmth effect of floss.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116219629B_ABST
    Figure CN116219629B_ABST
Patent Text Reader

Abstract

The present invention relates to a polyimide nanofiber flake and a preparation method thereof. The method comprises the following steps: (1) synthesizing a hot-melt polyamic acid spinning solution A using diamine and dianhydride monomers; (2) synthesizing a partially melted polyamic acid spinning solution B using diamine and dianhydride monomers; (3) electrospinning the spinning solution A and the spinning solution B to form a polyamic acid composite nanofiber membrane; (4) placing the polyamic acid composite nanofiber membrane between two insulating fiber webs and opening it with statically charged hot air to obtain a fluffy polyamic acid nanofiber flake; (5) subjecting the fluffy polyamic acid nanofiber flake to thermal imidization treatment to obtain a polyimide nanofiber flake with a multilayer structure. The method is simple in process and avoids dependence on environmental humidity. The flake has excellent windproof effect, warmth retention performance, compressibility and resilience, etc.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of thermal insulation materials for textiles, and in particular to polyimide nanofiber flakes and a preparation method thereof. Background Art

[0002] In recent years, high-performance fiber flakes have attracted more and more attention among the thermal insulation materials used in textiles (such as clothing, bedding, etc.). Flakes refer to fluffy sheets made of plant fibers, animal fibers or chemical fibers for warmth, heat insulation or shockproof. In the field of thermal insulation materials for textiles, flakes, as a loose filling material, have the advantages of light weight and warmth.

[0003] Among many high-performance fiber flake raw materials, polyimide has excellent properties such as high and low temperature resistance, flame retardancy, light weight, warmth retention, antibacterial, and far infrared, so the application field of its fiber flake products is expanding year by year, and the military and civilian markets are broad. However, this type of polyimide fiber flakes, due to its large fiber diameter and large pore size between fibers, is prone to air flow in it when there is wind and / or a large temperature difference between the inside and outside, causing heat loss, thereby reducing its warmth retention, and its insulation effect is average.

[0004] Nanofibers have a small diameter, and the resulting flakes have the characteristics of high porosity, small pore size, and light weight. They can store a large amount of still air, thereby improving the warmth and insulation effects, and have great application prospects in the field of thermal insulation flakes. However, the thickness of nanofiber flakes formed by electrospinning is usually less than 1 mm, which makes them poor in warmth retention, and their compressibility and resilience are poor, which greatly limits their practical application.

[0005] So far, there have been many reports on the research of nanofiber flakes. In one study, fiber flakes with both micron and nanometer sizes were obtained by electrospinning in a high humidity environment (usually with humidity greater than 80%). However, there is only slight bonding between the fibers, the structure is easy to collapse, the compressibility and resilience are poor, which affects its warmth retention, and there is also a phenomenon of flying flakes during the preparation process.

[0006] In addition, in another study, a gas supply device was introduced on the side of the electrospinning nozzle to introduce air during the electrospinning process, thereby obtaining fluffy nanofiber flakes. However, the airflow at the nozzle affects the stability of the spinning jet, and the obtained nanofibers are ordinary cylindrical, and the fluffy structure is simply piled up, unstable, and easy to collapse, which cannot guarantee long-term use.

[0007] Therefore, it is necessary to develop a method for preparing polyimide nanofiber flakes with simple process and large-scale production having excellent windproof effect, thermal insulation performance, compressibility and resilience to meet its application requirements in the field of thermal insulation materials. Summary of the invention

[0008] Technical issues

[0009] The first object of the present invention is to provide a method for preparing polyimide nanofiber flakes. The method is simple in process, can be rapidly mass-produced, and avoids dependence on ambient humidity.

[0010] The second object of the present invention is to provide a polyimide nanofiber flake with a multilayer structure, which has excellent windproof effect, warmth retention performance, compressibility and resilience, and can be used for a long time.

[0011] Technical Solution

[0012] According to a first aspect of the present invention, the present invention provides a method for preparing a polyimide nanofiber flake, the method comprising the following steps:

[0013] (1) using diamine and dianhydride monomers to synthesize hot-melt polyamic acid spinning solution A;

[0014] (2) using diamine and dianhydride monomers to synthesize a partially melted polyamic acid spinning solution B;

[0015] (3) electrospinning the hot-melt polyamic acid spinning solution A and the partially meltable polyamic acid spinning solution B to form a polyamic acid layer A and a polyamic acid layer B, respectively, and stacking them to form a polyamic acid composite nanofiber membrane, wherein the polyamic acid composite nanofiber membrane comprises a stacked combination of the polyamic acid layer A, the polyamic acid layer B and the polyamic acid layer A;

[0016] (4) placing the polyamic acid composite nanofiber membrane between two insulating fiber webs arranged horizontally and parallel to each other, allowing statically charged hot air to pass through the polyamic acid composite nanofiber membrane from the bottom to the top from below the two insulating fiber webs to loosen the polyamic acid composite nanofiber membrane, thereby obtaining fluffy polyamic acid nanofiber flakes;

[0017] (5) The fluffy polyamic acid nanofiber flakes are subjected to thermal imidization treatment to obtain polyimide nanofiber flakes with a multilayer structure.

[0018] In one embodiment, in step (1),

[0019] The diamine monomer is one or more of diaminodiphenyl ether diamine (ODA), all-meta-triphenyl diether diamine (1,3,3-APB), bisphenol A diamine (BAPP) and 4,4-diaminodiphenyl sulfone (DDS),

[0020] The dianhydride monomer is one or more of biphenyl dianhydride (BPDA), triphenyl diether dianhydride (HQPDA), diphenyl ether dianhydride (ODPA), benzophenone dianhydride (BTDA), bisphenol A dianhydride (BPADA) and diphenyl sulfide dianhydride (TDPA).

[0021] In one embodiment, in step (2),

[0022] The diamine monomer is a combination of a type I diamine monomer and a type II diamine monomer,

[0023] The type I diamine monomer is one or more of diaminodiphenyl ether diamine (ODA), all-meta-triphenyl diether diamine (1,3,3-APB) and bisphenol A diamine (BAPP),

[0024] The type II diamine monomer is one or more of p-phenylenediamine (PPD), biphenylenediamine (Bz) and 4,4-diamino-2,2-dimethylbiphenyl (DMB),

[0025] The dianhydride monomer is a combination of a type I dianhydride monomer and a type II dianhydride monomer,

[0026] The type I dianhydride monomer is one or more of triphenyl diether dianhydride (HQPDA), diphenyl ether dianhydride (ODPA), benzophenone dianhydride (BTDA) and bisphenol A dianhydride (BPADA),

[0027] The type II dianhydride monomer is one or more of biphenyl dianhydride (BPDA) and terephthalic anhydride (PMDA).

[0028] In one embodiment, in step (3), the electrospinning is performed by multiple groups of electrospinning spinnerets, wherein the multiple groups of electrospinning spinnerets include a three-layer spinning spinneret group.

[0029] The number of the upper layer spinning spinnerets is 1 to 3, the number of the bottom layer spinning spinnerets is 1 to 3, and the number of the middle layer spinning spinnerets is 3 to 20.

[0030] In one embodiment, in step (4),

[0031] The two insulating fiber nets are both aramid fiber nets, and the mesh size is 2 to 5 cm.

[0032] The distance between the two insulating fiber meshes is 5 to 30 mm.

[0033] The statically charged hot air is hot air with positive or negative charges, and the hot air temperature is 80-150°C.

[0034] In one embodiment, the temperature of the thermal imidization treatment is 300-450°C.

[0035] According to a second aspect of the present invention, the present invention provides a polyimide nanofiber flake prepared by the above method, wherein the flake comprises a superimide layer A, a polyimide layer B and a polyimide layer A.

[0036] Wherein, the density of the flakes is less than 5 mg / cm 3 , air permeability is less than 10mm / s, moisture permeability is greater than 6000g / (m 2 ·24h), compression rate is greater than 80%, and recovery rate is greater than 90%.

[0037] In one embodiment, the polyimide layer A is a film-like windproof layer, and the polyimide layer B is a fluffy thermal insulation layer.

[0038] In one embodiment, the polyimide layer A is obtained by thermal imidization of hot-melt polyamic acid, and the fiber diameter is 100 to 500 nm.

[0039] The thickness of the polyimide layer A is 1 to 100 μm.

[0040] The pore size of the polyimide layer A is 0.5-2 μm.

[0041] In one embodiment, the polyimide layer B is obtained by thermal imidization of partially molten polyamic acid, and the fiber diameter is 500 to 1500 nm.

[0042] The thickness of the polyimide layer B is 1 to 20 mm.

[0043] The pore size of the polyimide layer B is 3-10 μm.

[0044] Beneficial Effects

[0045] Compared with the prior art, the present invention has the following advantages.

[0046] (1) The preparation method of the present invention is not highly dependent on environmental humidity, and the electrospinning step (step 3) can be performed in a conventional electrospinning environment to obtain a polyamic acid composite nanofiber membrane. For example, the electrospinning step can be performed in a spinning environment with a temperature of 20 to 30° C. and a humidity of 30 to 50%.

[0047] That is to say, the present invention can avoid using special conditions such as a high humidity environment (humidity is usually greater than 80%) required by the prior art, so that no flying catkins will occur during the preparation process.

[0048] (2) The preparation method of the present invention adopts a specific opening step (step 4), wherein the polyamic acid composite nanofiber membrane is placed between two insulating fiber webs arranged horizontally and parallel to each other, and hot air with static electricity passes through the polyamic acid composite nanofiber membrane, so that the composite nanofiber membrane is opened under the synergistic effect of electrostatic repulsion and strong wind force, thereby obtaining fluffy polyamic acid nanofiber flakes. In addition, the degree of opening of the flakes can be easily controlled by adjusting the distance between the two insulating fiber webs.

[0049] (3) The preparation method of the present invention is simple to operate, can be formed in one step, and can be easily implemented in large-scale production.

[0050] (4) The polyimide nanofiber flakes of the present invention comprise a specific multilayer structure, wherein the multilayer structure comprises a stacked combination of a polyimide layer A, a polyimide layer B, and a polyimide layer A.

[0051] The polyimide layer A as the upper layer and the bottom layer is obtained by thermal imidization of hot-melt polyamic acid. During the thermal imidization, the hot-melt polyamic acid melts to form a porous fiber mesh with a small pore size, thereby having an excellent windproof effect.

[0052] The polyimide layer B as the middle layer is obtained by the thermal imidization treatment of partially molten polyamic acid. During the thermal imidization treatment, the fiber overlap points in the partially molten polyamic acid will melt and bond during the imidization process, which increases the support points for elastic rebound for the flakes and has a mutually cross-linked three-dimensional network structure. That is, the polyimide layer B has a fluffy structure with high compressibility and resilience, so that the flakes have high compressibility and resilience. As a result, the flakes will not collapse significantly after being subjected to external force, and the static air content is increased, thereby improving the warmth retention effect. BRIEF DESCRIPTION OF THE DRAWINGS

[0053] Figure 1 Schematic diagram of the structure of a polyimide nanofiber flake according to one embodiment of the present invention.

[0054] Figure 2a This is a SEM image of the polyimide layer A (upper layer) of the polyimide nanofiber flakes of Example 1.

[0055] Figure 2b This is a SEM image of the polyimide layer B (middle layer) of the polyimide nanofiber flakes of Example 1.

[0056] Figure 2c This is the SEM image of the polyimide layer A (bottom layer) of the polyimide nanofiber flakes of Example 1.

[0057] Reference numerals

[0058] 10 Polyimide layer A (upper layer)

[0059] 20 Polyimide layer B (middle layer)

[0060] 30 Polyimide layer A (bottom layer) DETAILED DESCRIPTION

[0061] Hereinafter, the present invention will be described in detail with reference to the accompanying drawings. The terms or words used in this specification and claims should not be restrictively interpreted as common or dictionary definitions, and should be interpreted as meanings and concepts corresponding to the technical ideas of the present invention on the basis that the inventor can appropriately define the concepts of the terms to describe the principles of the invention in the best possible way.

[0062] When the conditions and methods for measuring a property or parameter described in this specification are not described in detail, the property or parameter is measured using the measurement conditions and methods generally used by those skilled in the art.

[0063] Unless otherwise specified, "%" used herein means % by weight.

[0064] Method for preparing polyimide nanofiber flakes

[0065] The present invention provides a method for preparing a polyimide nanofiber flake, the method comprising the following steps:

[0066] (1) using diamine and dianhydride monomers to synthesize hot-melt polyamic acid spinning solution A;

[0067] (2) using diamine and dianhydride monomers to synthesize a partially melted polyamic acid spinning solution B;

[0068] (3) electrospinning the hot-melt polyamic acid spinning solution A and the partially meltable polyamic acid spinning solution B to form a polyamic acid layer A and a polyamic acid layer B, respectively, and stacking them to form a polyamic acid composite nanofiber membrane, wherein the polyamic acid composite nanofiber membrane comprises a stacked combination of the polyamic acid layer A, the polyamic acid layer B and the polyamic acid layer A;

[0069] (4) placing the polyamic acid composite nanofiber membrane between two insulating fiber webs arranged horizontally and parallel to each other, allowing statically charged hot air to pass through the polyamic acid composite nanofiber membrane from the bottom to the top from below the two insulating fiber webs to loosen the polyamic acid composite nanofiber membrane, thereby obtaining fluffy polyamic acid nanofiber flakes;

[0070] (5) subjecting the fluffy polyamic acid nanofiber flakes to thermal imidization treatment to obtain a polyimide nanofiber flake with a multilayer structure

[0071] In the following, each step will be described in detail.

[0072] Step (1): Synthesis of Spinning Solution A

[0073] Diamine and dianhydride monomers are used to synthesize the hot-melt polyamic acid spinning solution A. Suitable diamine and dianhydride monomers can be determined according to conventional selection.

[0074] The diamine monomer is a compound containing two amino groups and is a conventional component for preparing polyamic acid spinning solution. The diamine monomer may be one or more of diaminodiphenyl ether diamine (ODA), all-meta-triphenyl diether diamine (1,3,3-APB), bisphenol A diamine (BAPP) and 4,4-diaminodiphenyl sulfone (DDS).

[0075] The dianhydride monomer is a compound containing two carboxylic anhydride groups and is a conventional component for preparing polyamic acid spinning solution. The dianhydride monomer can be one or more of biphenyl dianhydride (BPDA), triphenyl diether dianhydride (HQPDA), diphenyl ether dianhydride (ODPA), benzophenone dianhydride (BTDA), bisphenol A dianhydride (BPADA) and diphenyl sulfide dianhydride (TDPA).

[0076] The hot-melt polyamic acid spinning solution A is used to prepare the polyamic acid layer A as the bottom layer and the upper layer, which is completely melted during the subsequent thermal imidization treatment to form a polyimide layer A with small pores (which is a porous fiber web).

[0077] Step (2): Synthesis of Spinning Solution B

[0078] The partially melted polyamic acid spinning solution B is synthesized using diamine and dianhydride monomers. Suitable diamine and dianhydride monomers can be determined according to conventional selection.

[0079] For example, the diamine monomer may be a combination of a type I diamine monomer and a type II diamine monomer.

[0080] The type I diamine monomer may be one or more of diaminodiphenyl ether diamine (ODA), all-meta-triphenyl diether diamine (1,3,3-APB) and bisphenol A diamine (BAPP).

[0081] The type II diamine monomer may be one or more of p-phenylenediamine (PPD), biphenylenediamine (Bz) and 4,4-diamino-2,2-dimethylbiphenyl (DMB).

[0082] The dianhydride monomer may be a combination of a type I dianhydride monomer and a type II dianhydride monomer.

[0083] The type I dianhydride monomer may be one or more of triphenyl diether dianhydride (HQPDA), diphenyl ether dianhydride (ODPA), benzophenone dianhydride (BTDA) and bisphenol A dianhydride (BPADA).

[0084] The type II dianhydride monomer may be one or more of biphenyl dianhydride (BPDA) and terephthalic anhydride (PMDA).

[0085] The partially melted polyamic acid spinning solution B is used to prepare a polyamic acid layer B as an intermediate layer, which is partially melted during the subsequent thermal imidization treatment to form a fluffy polyimide layer B having a mutually cross-linked three-dimensional network structure.

[0086] In the present invention, there is no particular limitation on the order of performing steps (1) and (2). For example, steps (1) and (2) may be performed simultaneously; or step (1) may be performed first, and then step (2); or step (2) may be performed first, and then step (1).

[0087] Step (3): Electrospinning (electrospinning)

[0088] The hot-melt polyamic acid spinning solution A and the partially meltable polyamic acid spinning solution B are electrospun to form a polyamic acid layer A and a polyamic acid layer B, respectively, and they are stacked to form a polyamic acid composite nanofiber membrane, wherein the polyamic acid composite nanofiber membrane comprises a superimposed combination of a polyamic acid layer A, a polyamic acid layer B and a polyamic acid layer A.

[0089] Electrospinning is a simple and effective technology for producing micron to nanometer-scale fibers. It allows electrostatically charged polymer solutions to flow and deform in an electrostatic field, solidify through solvent evaporation, and form fibrous substances. Continuous nanofibers (filament nanofibers) can be prepared simply and effectively by electrospinning. Filaments, also known as continuous filaments, are a type of chemical fiber, usually smooth and shiny continuous threads that are several meters to several kilometers long. There is no limit to the length of the filaments, which can be determined as needed.

[0090] The electrospinning can be performed continuously by multiple groups of electrospinning spinnerets. For example, polyamic acid spinning solution A and polyamic acid spinning solution B can be electrospun separately by multiple groups of electrospinning spinnerets arranged in sequence in a line, so that they fall on a conductive metal belt (such as a stainless steel belt) in sequence, thereby obtaining the polyamic acid composite nanofiber membrane.

[0091] There is no limitation on the length of the polyamic acid composite nanofiber membrane, and it can be any length, for example, more than 1 m, more than 10 m, more than 100 m, or more than 1000 m.

[0092] There is no limit to the width of the polyamic acid composite nanofiber membrane, which can be adjusted by the width of the conductive metal tape or by subsequent cutting.

[0093] The thickness of the polyamic acid composite nanofiber membrane can be determined as needed, and can generally be 0.1 to 1 mm.

[0094] In one embodiment, the plurality of groups of electrospinning spinnerets may include three layers of spinning spinneret groups, wherein the number of groups of the upper layer spinning spinnerets may be 1 to 3, the number of groups of the bottom layer spinning spinnerets may be 1 to 3, and the number of groups of the middle layer spinning spinnerets may be 3 to 20, preferably 5 to 15, and more preferably 7 to 11. The ratio of the polyimide layer A and the polyimide layer B in the flakes and the weight of the flakes may be adjusted by the number of groups of the spinning spinnerets.

[0095] There is no specific restriction on the number of stacked layers of polyamic acid layer A and polyamic acid layer B in the polyamic acid composite nanofiber membrane, as long as polyamic acid layer A and polyamic acid layer B are alternately stacked and the upper and bottom layers (i.e., the two outermost layers) are both polyamic acid layer A.

[0096] For example, the polyamic acid composite nanofiber membrane can be a three-layer combination (ABA combination) of polyamic acid layer A, polyamic acid layer B and polyamic acid layer A stacked in sequence, or a five-layer combination (ABABA combination) of polyamic acid layer A, polyamic acid layer B, polyamic acid layer A, polyamic acid layer B and polyamic acid layer A stacked in sequence, etc.

[0097] Step (4): Loosening

[0098] The polyamic acid composite nanofiber membrane is placed between two insulating fiber nets arranged horizontally and parallel to each other, and statically charged hot air is passed through the polyamic acid composite nanofiber membrane from bottom to top from below the two insulating fiber nets to loosen it, thereby obtaining fluffy polyamic acid nanofiber flakes.

[0099] The length and width of the polyamic acid composite nanofiber membrane obtained in step (3) can be appropriately cut to be smaller than the length and width of the insulating fiber web, respectively, so as to be suitable for placement between two insulating fiber webs.

[0100] Specifically, two insulating fiber nets are arranged horizontally and parallel to each other. Then, a nanofiber membrane is placed between the two insulating fiber nets, and the nanofiber membrane is located on the lower insulating fiber net due to gravity. Then, hot air with static electricity is passed through the two insulating fiber nets from bottom to top to loosen the nanofiber membrane between them to a fluffy state.

[0101] The insulating fiber mesh is used to allow hot air to pass through and fix the loosened flakes. The insulating fiber mesh can be, for example, an aramid fiber mesh or a Teflon fiber mesh, which does not deform when statically charged hot air passes through, and does not cause charge loss of the composite nanofiber membrane. The length, width and thickness of the insulating fiber mesh can be determined according to conventional selections, for example, the length can be 1 to 10 m, the width can be 0.2 to 2 m, and the thickness can be 0.2-2 mm. The mesh size of the insulating fiber mesh can be 2 to 5 cm, preferably 2.2 to 4 cm, and more preferably 2.5 to 3 cm.

[0102] The composite nanofiber membrane is opened into fluffy polyamic acid nanofiber flakes under the synergistic effect of the electrostatic repulsion of the electrostatic hot air and the strong wind force, and fills the space between the two insulating fiber nets.

[0103] The opening refers to expanding the polyamic acid composite nanofiber membrane (i.e., increasing the volume) to form fluffy polyamic acid nanofiber flakes. Generally, the volume of the fluffy polyamic acid nanofiber flakes obtained after opening can be 20 to 150 times, preferably 30 to 100 times, and more preferably 40 to 60 times the volume of the polyamic acid composite nanofiber membrane before opening. The fluffy flakes can store a large amount of still air, which is conducive to achieving excellent warmth retention effect.

[0104] By setting the distance between the two insulating fiber webs, the degree of opening of the nanofiber flakes can be controlled. For example, the distance between the two insulating fiber webs can be 5 to 30 mm, such as 6 to 20 mm, or 8 to 12 mm. The distance can be appropriately determined according to the weight of the flakes to help maintain the appropriate fluffiness and molding thickness of the flakes. If the above distance is too small, the flakes may not be fluffy enough and the warmth retention effect may be poor. If the above distance is too large, the flakes may be difficult to form.

[0105] The electrostatically charged hot air can be hot air with positive or negative charges, and the existence of the charges makes the fibers in the nanofiber membrane have the same charge. The fibers with the same charge will be separated from each other due to the electrostatic repulsion.

[0106] In addition, hot air will further volatilize the residual solvent in the fiber membrane, which is conducive to further opening. The hot air temperature can be 80-150°C, preferably 90-130°C, and more preferably 100-120°C. If the hot air temperature is too low, the residual solvent in the fiber membrane may not be completely volatilized, affecting its degree of opening. If the hot air temperature is too high, the hot-melt polyamic acid nanofibers may be initially melted, which will also affect the opening of the fiber membrane.

[0107] The pressure and air volume of the hot air can be appropriately determined as needed. For example, the hot air can be positive pressure, the pressure can be 100-600 Pa, preferably 200-500 Pa, more preferably 300-400 Pa. The air volume can be 2000-10000 m 3 / h, preferably 3000~8000m 3 / h, more preferably 4000-6000m 3 / h. If the hot air pressure or air volume is too low, the force is too weak, the fiber membrane does not expand enough, resulting in insufficient opening, which affects the fluffiness of the flakes. If the hot air pressure or air volume is too high, the fiber membrane is easily blown apart, making it difficult for the flakes to form.

[0108] Step (5): Thermal imidization

[0109] The fluffy polyamic acid nanofiber flakes are subjected to thermal imidization treatment to obtain a polyimide nanofiber flake with a multilayer structure. Specifically, the flakes include a superimide layer A, a polyimide layer B, and a polyimide layer A. The polyimide layer A is obtained by thermal imidization treatment of the polyamic acid layer A, and the polyimide layer B is obtained by thermal imidization treatment of the polyamic acid layer B.

[0110] Thermal imidization refers to the dehydration and cyclization of polyamic acid at high temperature to obtain polyimide, which is a common step for preparing polyimide.

[0111] Through the thermal imidization treatment, the polyamic acid flakes can be dehydrated and cyclized to obtain polyimide flakes. In addition, through the thermal imidization treatment, the polyamic acid layer A as the bottom layer and the upper layer can be made into a porous fiber net with a small pore size (for example, a pore size of 0.5 to 2 μm) after the thermal imidization treatment, which has a good windproof effect; and the polyamic acid layer B as the middle layer is partially melted to form a cross-linked three-dimensional network fluffy structure, which can contain a large amount of static air, thereby having excellent warmth retention, compressibility and resilience.

[0112] The temperature of thermal imidization can be 300-450°C. If the temperature is too low, the imidization of the polyamic acid may not be complete, the thermal melting of the polyamic acid layer A is insufficient, the pore size of the obtained polyimide layer A is too large, and the crosslinking of the polyamic acid layer B is insufficient, the compressibility and resilience of the obtained polyimide layer B are poor, affecting the thermal insulation performance. If the temperature is too high, the polyimide will degrade, the crosslinking of the polyamic acid layer B is excessive, and the fluffy structure collapses, which will also affect the thermal insulation performance.

[0113] Polyimide nanofiber flakes

[0114] The present invention also provides a polyimide nanofiber flake, which comprises a superimposed combination of a polyimide layer A, a polyimide layer B and a polyamic acid layer A, wherein the density of the flake is less than 5 mg / cm 3 , air permeability is less than 10mm / s, moisture permeability is greater than 6000g / (m 2 · 24h), the compression rate is greater than 80%, and the recovery rate is greater than 90%. The polyimide nanofiber flakes can be prepared by the above method of the present invention.

[0115] In one embodiment, the polyimide layer A as the upper layer and the bottom layer is a film-like windproof layer, and the polyimide layer B as the middle layer is a fluffy thermal insulation layer.

[0116] There is no specific limitation on the number of stacked layers of polyimide layer A and polyimide layer B in the polyimide nanofiber flakes, as long as polyimide layer A and polyimide layer B are alternately stacked and the upper and bottom layers (i.e., the two outermost layers) are both polyimide layer A.

[0117] For example, the polyimide composite nanofiber flakes may be a three-layer combination of a polyimide layer A, a polyimide layer B, and a polyimide layer A stacked in sequence (ie, an ABA combination, such as Figure 1 As described above), or a five-layer combination of polyimide layer A, polyimide layer B, polyimide layer A, polyimide layer B and polyimide layer A stacked in sequence (ie, ABABA combination), etc.

[0118] The flake density can be measured as follows: first, measure its surface density according to GB / T 24218.1-2009 (Test methods for textile nonwovens Part 1: Determination of mass per unit area); then, measure its thickness according to GB / T24218.2-2009 (Test methods for textile nonwovens Part 2: Determination of thickness); then, divide the surface density by the thickness to obtain the density.

[0119] The air permeability of the flakes can be measured according to GB / T 5453-1997 (Determination of air permeability of textile fabrics).

[0120] The water vapor permeability of the flakes can be measured according to GB / T 12704.2-2009 (Test method for water vapor permeability of textile fabrics Part 2: Evaporation method).

[0121] The compression rate and resilience rate of the flakes can be measured according to the test method in Appendix A of FZ / T 64003-2021 (Spray-bonded cotton flakes).

[0122] In one embodiment, the polyimide layer A is obtained by thermal imidization of hot-melt polyamic acid.

[0123] The fiber diameter in the polyimide layer A can be 100-500 nm, preferably 150-400 nm, more preferably 200-400 nm, and most preferably 200-300 nm. If the fiber diameter is less than 100 nm, the fiber is too densely packed, and the pore size of the fiber membrane after hot melting is low, resulting in poor moisture permeability; if the fiber diameter is higher than 500 nm, the fiber is too loosely packed, and the pore size of the fiber membrane after hot melting is large, resulting in high air permeability and poor windproof effect.

[0124] The thickness of the polyimide layer A can be 1 to 100 μm, preferably 10 to 80 μm, more preferably 10 to 50 μm, and most preferably 20 to 30 μm. If the thickness of the polyimide layer A is less than 1 μm, the windproof layer has a poor windproof effect; if the thickness of the polyimide layer A is greater than 100 μm, the windproof layer is too thick, which easily leads to too low moisture permeability, thereby poor comfort.

[0125] The pore size of the polyimide layer A can be 0.5 to 2 μm, preferably 0.8 to 1.8 μm, more preferably 1 to 1.5 μm, and most preferably 0.8 to 1.2 μm. If the pore size of the polyimide layer A is less than 0.5 μm, the moisture permeability is poor; if the pore size of the polyimide layer A is greater than 2 μm, the air permeability is high and the windproof effect is poor.

[0126] In one embodiment, the polyimide layer B is obtained by thermal imidization of a partially melt-type polyamic acid.

[0127] The fiber diameter in the polyimide layer B can be 500-1500nm, preferably 700-1400nm, more preferably 800-1200nm, and most preferably 900-1100nm. If the fiber diameter is less than 500nm, the flakes are not fluffy enough after opening, and the static air retention is not enough, resulting in poor thermal insulation performance; if the fiber diameter is greater than 1500nm, the flakes have a larger pore size after opening, which easily causes air to flow through them, resulting in heat loss, and thus reducing their thermal insulation performance.

[0128] The thickness of the fiber membrane can be 1 to 20 mm, preferably 3 to 17 mm, more preferably 4 to 13 mm, and most preferably 5 to 10 mm. If the thickness of the polyimide layer B is less than 1 mm, the amount of still air retention is insufficient, resulting in poor warmth retention; if the thickness of the polyimide layer B is greater than 20 mm, the wadding is too bulky and the wearing comfort is poor.

[0129] The pore size of the fiber membrane can be 3 to 10 μm, preferably 4 to 9 μm, more preferably 5 to 8 μm, and most preferably 5 to 6 μm. If the pore size of the polyimide layer B is less than 3 μm, the porosity of the flakes is low, the fluffiness is not enough, the static air retention is insufficient, and the thermal insulation performance is poor; if the pore size of the polyimide layer B is greater than 10 μm, it is easy to cause air to flow through it, causing heat loss, thereby reducing its thermal insulation performance.

[0130] Example

[0131] Hereinafter, the present invention will be described in detail with reference to embodiments to specifically describe the present invention. However, embodiments of the present invention may be modified into various other forms, and the scope of the present invention should not be construed as being limited to the embodiments described below. Embodiments of the present invention are provided to more fully describe the present invention to those of ordinary skill in the art.

[0132] The experimental methods in the following examples, unless otherwise specified, are generally conventional conditions in the art or conditions recommended by the manufacturer; the raw materials and equipment used are all commercially available from conventional markets, etc., unless otherwise specified.

[0133] The following is based on the same surface density (also known as gram weight, g / m 2 )Prepare polyimide nanofiber flakes of Examples 1 to 6 and Comparative Examples 1 to 4, and compare their thermal insulation properties and other properties.

[0134] Example 1

[0135] The polyimide nanofiber flakes were prepared by the following steps.

[0136] Step (1): Synthesis of Spinning Solution A

[0137] 410.5 g (1 mol) of bisphenol A diamine (BAPP) and 294.2 g (1 mol) of biphenyl dianhydride (BPDA) were prepared in a molar ratio of 1:1, and 3993.3 g of solvent N,N-dimethylacetamide (DMAC) was also prepared. They were stirred in a polymerization reactor for 10 hours to obtain a hot-melt polyamic acid spinning solution A with a mass fraction of 15%.

[0138] Step (2): Synthesis of Spinning Solution B

[0139] 120.1g (0.6mol) of diphenyl ether diamine (ODA), 297.2g (1.4mol) of 4,4-diamino-2,2-dimethylbiphenyl (DMB), 261.7g (1.2mol) of pyromellitic dianhydride (PMDA) and 321.8g (0.8mol) of triphenyl diether dianhydride (HQPDA) were prepared in a molar ratio of 0.3:0.7:0.6:0.4, and 4560g of solvent N,N-dimethylacetamide (DMAC) was prepared. They were stirred in a polymerization reactor for 12h to obtain a partially melted polyamic acid spinning solution B with a mass fraction of 18%.

[0140] Step (3): Electrospinning (electrospinning)

[0141] Ten groups of electrospinning spinnerets are arranged in sequence on a line to electrospin the hot-melt polyamic acid spinning solution A and the partially meltable polyamic acid spinning solution B.

[0142] The hot-melt polyamic acid spinning solution A was electrospun in an electric field with an electric field strength of 25 KV / m through the front and rear groups of spinnerets, and the partially molten polyamic acid spinning solution B was electrospun in an electric field with an electric field strength of 30 KV / m through the middle 8 groups of spinnerets.

[0143] The polyamic acid layer A and polyamic acid layer B formed by electrospinning fall on a conductive stainless steel belt moving at a speed of 0.1 m / min in sequence. After electrospinning for 35 min, a polyamic acid composite nanofiber membrane with a three-layer structure of polyamic acid layer A / polyamic acid layer B / polyamic acid layer A is formed with a length of 3.5 m, a width of 0.9 m, and a thickness of 260 μm.

[0144] Step (4): Loosening

[0145] Two aramid fiber nets were prepared, each of which had a length of 4 m, a width of 0.95 m, a thickness of 1 mm, and a mesh size of 3 cm.

[0146] The polyamic acid nanofiber membrane is placed between the two aramid fiber nets. The aramid fiber nets are arranged horizontally and parallel to each other, and the fixed distance between the fiber nets is 10 mm.

[0147] Make the air volume 4200m 3 / h, a pressure of 350Pa, and a temperature of 80°C, positively charged hot air passes through the composite nanofiber membrane from bottom to top from the bottom of the aramid fiber web, loosening it and filling the space between the two aramid fiber webs to obtain a 10mm thick fluffy polyamic acid nanofiber flakes.

[0148] Step (5): Thermal imidization

[0149] The fluffy polyamic acid nanofiber flakes are fed into a 5m long chain furnace for thermal imidization treatment. The chain furnace has five temperature zones, the temperatures from the inlet end to the outlet end are 100-390°C, and the flakes move at a speed of 1m / min.

[0150] After imidization treatment, a three-layer polyimide nanofiber flake was obtained with a surface density of 15 g / m 2 , density is 3mg / cm 3 , thickness is 5mm.

[0151] Example 2 (Using different monomers from Example 1 to prepare spinning solutions A and B)

[0152] The polyimide nanofiber flakes were prepared by the same steps as in Example 1, except for the following steps.

[0153] Step (1): Synthesis of Spinning Solution A

[0154] 200.2 g (1 mol) of diphenyl ether diamine (ODA) and 322.2 g (1 mol) of benzophenone dianhydride (BTDA) were prepared at a molar ratio of 1:1, and 2960.3 g of solvent N,N-dimethylacetamide (DMAC) was also prepared. They were stirred in a polymerization reactor for 10 hours to obtain a hot-melt polyamic acid spinning solution A with a mass fraction of 15%.

[0155] Step (2): Synthesis of Spinning Solution B

[0156] 320.4g (1.6mol) of diphenyl ether diamine (ODA), 84.9g (0.4mol) of 4,4-diamino-2,2-dimethylbiphenyl (DMB), 305.4g (1.4mol) of pyromellitic dianhydride (PMDA) and 312.3g (0.6mol) of bisphenol A diether dianhydride (BPADA) were prepared in a molar ratio of 0.8:0.2:0.7:0.3, and 4506.7g of solvent N,N-dimethylacetamide (DMAC) were prepared. They were stirred in a polymerization reactor for 12 hours to obtain a partially melted polyamic acid spinning solution B with a mass fraction of 18.5%.

[0157] The surface density of the obtained flakes is 15g / m 2 , density is 3mg / cm 3 , thickness is 5mm.

[0158] Example 3 (Using different monomers from Example 1 to prepare spinning solutions A and B)

[0159] The polyimide nanofiber flakes were prepared by the same steps as in Example 1, except for the following steps.

[0160] Step (1): Synthesis of Spinning Solution A

[0161] 410.5 g (1 mol) of bisphenol A diamine (BAPP) and 402.3 g (1 mol) of triphenylene ether dianhydride (HQPDA) were prepared in a molar ratio of 1:1, and 4642.3 g of solvent N,N-dimethylacetamide (DMAC) was also prepared. They were stirred in a polymerization reactor for 10 hours to obtain a hot-melt polyamic acid spinning solution A with a mass fraction of 14.9%.

[0162] Step (2): Synthesis of Spinning Solution B

[0163] 160.2g (0.8mol) of diphenyl ether diamine (ODA), 221.1g (1.2mol) of biphenyl diamine (Bz), 500.2g (1.7mol) of biphenyl dianhydride (BPDA) and 120.7g (0.3mol) of triphenyl diether dianhydride (HQPDA) were prepared in a molar ratio of 0.4:0.6:0.85:0.15, and 4272.5g of solvent N,N-dimethylacetamide (DMAC) was prepared. They were stirred in a polymerization reactor for 12 hours to obtain a partially melted polyamic acid spinning solution B with a mass fraction of 19%.

[0164] The surface density of the obtained flakes is 15g / m 2 , density is 3mg / cm 3 , thickness is 5mm.

[0165] Example 4 (Using different monomers from Example 1 to prepare spinning solutions A and B)

[0166] The polyimide nanofiber flakes were prepared by the same steps as in Example 1, except for the following steps.

[0167] Step (1): Synthesis of Spinning Solution A

[0168] 200.2 g (1 mol) of diphenyl ether diamine (ODA) and 402.3 g (1 mol) of triphenyl ether dianhydride (HQPDA) were prepared at a molar ratio of 1:1, and 3335.4 g of solvent N,N-dimethylacetamide (DMAC) was also prepared. They were stirred in a polymerization reactor for 10 hours to obtain a hot-melt polyamic acid spinning solution A with a mass fraction of 15.3%.

[0169] Step (2): Synthesis of Spinning Solution B

[0170] 200.2g (1 mol) of diphenyl ether diamine (ODA), 212.3g (1 mol) of 4,4-diamino-2,2-dimethylbiphenyl (DMB), 193.3g (0.6 mol) of benzophenone dianhydride (BTDA) and 305.4g (1.4 mol) of pyromellitic dianhydride (PMDA) were prepared in a molar ratio of 0.5:0.5:0.3:0.7, and 3810g of solvent N,N-dimethylacetamide (DMAC) were prepared. They were stirred in a polymerization reactor for 12 hours to obtain a partially melted polyamic acid spinning solution B with a mass fraction of 19.3%.

[0171] The surface density of the obtained flakes is 15g / m 2 , density is 2.5mg / cm 3 , thickness is 6mm.

[0172] Example 5 (Using different monomers from Example 1 to prepare spinning solutions A and B)

[0173] The polyimide nanofiber flakes were prepared by the same steps as in Example 1, except for the following steps.

[0174] Step (1): Synthesis of Spinning Solution A

[0175] 200.2 g (1 mol) of diphenyl ether diamine (ODA) and 520.5 g (1 mol) of bisphenol A diether dianhydride (BPADA) were prepared in a molar ratio of 1:1, and 4052.1 g of solvent N,N-dimethylacetamide (DMAC) was prepared. They were stirred in a polymerization reactor for 10 hours to obtain a hot-melt polyamic acid spinning solution A with a mass fraction of 15.1%.

[0176] Step (2): Synthesis of Spinning Solution B

[0177] 40g (0.2mol) of diphenyl ether diamine (ODA), 382.1g (1.8mol) of 4,4-diamino-2,2-dimethylbiphenyl (DMB), 248.2g (0.8mol) of diphenyl ether dianhydride (ODPA) and 261.7g (1.2mol) of pyromellitic dianhydride (PMDA) were prepared in a molar ratio of 0.1:0.9:0.4:0.6, and 4160.9g of solvent N,N-dimethylacetamide (DMAC) was prepared. They were stirred in a polymerization reactor for 12h to obtain a partially melted polyamic acid spinning solution B with a mass fraction of 18.3%.

[0178] The obtained flakes have a surface density of 15 g / m2, a density of 3 mg / cm3 and a thickness of 5 mm.

[0179] Example 6 (Using different monomers from Example 1 to prepare spinning solution B)

[0180] The polyimide nanofiber flakes were prepared by the same steps as in Example 1, except for the following steps.

[0181] Step (2): Synthesis of Spinning Solution B

[0182] 175.4g (0.6mol) 1,3,3-triphenyl diether diamine (1,3,3-APB), 297.2g (1.4mol) 4,4-diamino-2,2-dimethylbiphenyl (DMB), 156.1g (0.3mol) bisphenol A diether dianhydride (BPADA) and 370.8g (1.7mol) pyromellitic acid dianhydride (PMDA) were prepared in a molar ratio of 0.3:0.7:0.15:0.85, and 4317g solvent N,N-dimethylacetamide (DMAC) was prepared. They were stirred in a polymerization reactor for 12 hours to obtain a partially melted polyamic acid spinning solution B with a mass fraction of 18.8%.

[0183] The surface density of the obtained flakes is 15g / m 2 , density is 3mg / cm 3 , thickness is 5mm.

[0184] Comparative Example 1 (Step (4) (opening step) omitted)

[0185] The polyimide nanofiber flakes were prepared by the same steps as in Example 1, except that step (4) (opening step) was omitted.

[0186] The surface density of the obtained flakes is 15g / m 2 , density is 300mg / cm 3 , thickness is 0.05mm.

[0187] Comparative Example 2 (using only spinning solution B without using spinning solution A)

[0188] Polyimide nanofiber flakes were prepared by the same steps as in Example 1, except that step (1) was omitted and the 10 groups of electrospinning spinnerets in step (3) all subjected the spinning solution B to electrospinning in an electric field with an electric field strength of 30 KV / m.

[0189] The surface density of the obtained flakes is 15g / m 2 , density is 2.5mg / cm 3 , thickness is 6mm.

[0190] Comparative Example 3 (using only spinning solution A without using spinning solution B)

[0191] Polyimide nanofiber flakes were prepared by the same steps as in Example 1, except that step (2) was omitted and the 10 groups of electrospinning spinnerets in step (3) all subjected the spinning solution A to electrospinning in an electric field with an electric field strength of 25 KV / m.

[0192] The surface density of the obtained flakes is 15g / m 2 , density is 1000mg / cm 3 , with a thickness of 0.015 mm. Comparative Example 4 (the stacking combination in step (3) is changed to BAB)

[0193] The polyimide nanofiber flakes were prepared by the same steps as in Example 1, except for the following step (3).

[0194] Step (3): Electrospinning

[0195] Ten groups of electrospinning spinnerets are arranged in sequence on a line to electrospin the hot-melt polyamic acid spinning solution A and the partially meltable polyamic acid spinning solution B.

[0196] The partially molten polyamic acid spinning solution B was electrospun in an electric field with an electric field strength of 25 KV / m through the front 4 groups of spinnerets and the back 4 groups of spinnerets, and the hot-melt polyamic acid spinning solution A was electrospun in an electric field with an electric field strength of 30 KV / m through the middle 2 groups of spinnerets.

[0197] The polyamic acid layer B and polyamic acid layer A formed by electrospinning fall on a conductive stainless steel belt moving at a speed of 0.1 m / min in sequence. After electrospinning for 35 min, a polyamic acid composite nanofiber membrane with a three-layer structure of polyamic acid layer B / polyamic acid layer A / polyamic acid layer B is formed with a length of 3.5 m, a width of 0.9 m, and a thickness of 260 μm.

[0198] The surface density of the obtained flakes is 15g / m 2 , density is 3mg / cm 3 , thickness is 5mm.

[0199] Experimental Example 1: Using a scanning electron microscope to observe the morphology of the flakes

[0200] A scanning electron microscope (TESCAN, model VEGA3) was used to observe the microstructure of the polyimide nanofiber flakes obtained in Example 1 according to GB / T36422-2018 (Scanning electron microscopy method for determination of micromorphology and diameter of chemical fibers). Figure 2a to 2c As shown. Among them,

[0201] Figure 2a is the SEM image of the upper polyimide layer A.

[0202] Figure 2b This is the SEM image of the middle polyimide layer B.

[0203] Figure 2c This is the SEM image of the bottom polyimide layer A.

[0204] from Figure 2a and 2c It can be seen that the nanofibers in the upper and bottom polyimide layers A have been obviously melted and formed a fiber mesh with a smaller pore size, which makes it have a better windproof effect.

[0205] from Figure 2b It can be seen that the nanofibers in the middle polyimide layer B are in a mutually cross-linked three-dimensional network structure, which can store a large amount of static air and are partially melt-bonded at the fiber overlap points, increasing the support points for elastic rebound, so that the flakes have higher compressibility and resilience, and will not collapse significantly under the action of external force.

[0206] Experimental Example 2 Measurement of thermal insulation performance

[0207] Based on the same surface density (also known as gram weight, g / m 2 ) The thermal insulation performance of the flakes of Examples 1 to 6 and Comparative Examples 1 to 4 is compared. The thermal insulation performance of the flakes is expressed by the Crowe value, which can be measured according to GB / T11048-2008 (Determination of thermal resistance and moisture resistance of textiles under steady-state conditions for physiological comfort).

[0208] Specifically, the Crowe values ​​of the polyimide nanofiber flakes of Examples 1 to 6 and Comparative Examples 1 to 4 were measured using a fabric thermal insulation performance tester (Wenzhou Darong Textile Instrument Co., Ltd., Model YG(B)606E) according to GB / T 11048-2018. The results are shown in Table 1 below.

[0209] Table 1: Crosby values ​​of polyimide nanofiber flakes

[0210] <![CDATA[Clo value (unit: m 2 ·K / W)]]> Example 1 0.7 Example 2 0.76 Example 3 0.62 Example 4 0.75 Example 5 0.78 Example 6 0.69 Comparative Example 1 0.1 Comparative Example 2 0.5 Comparative Example 3 0.05 Comparative Example 4 0.52

[0211] As can be seen from Table 1, the polyimide nanofiber flakes of Examples 1 to 6 prepared by the method of the present invention have significantly larger Crowe values, indicating that the warmth retention effect is excellent.

[0212] In particular, it can be seen from the Crowe values ​​of the flakes of Example 1 and Comparative Example 1 that the opening step can significantly improve the warmth retention of the resulting flakes;

[0213] It can be seen from the clo values ​​of the wadding of Example 1 and Comparative Example 2 that the windproof layer can lock in the still air and further improve the warmth retention;

[0214] It can be seen from the flake cro values ​​of Example 1 and Comparative Example 3 that the polyimide layer B as a fluffy thermal insulation layer can store a large amount of static air and significantly improve the thermal insulation performance;

[0215] It can be seen from the lint values ​​of Example 1 and Comparative Example 4 that the polyimide layer A as a windproof layer can better lock the still air on the outer layer, thereby improving the warmth retention.

[0216] Experimental Example 3 Measurement of air permeability and moisture permeability

[0217] The air permeability of the polyimide nanofiber flakes of Examples 1 to 6 and Comparative Examples 1 to 4 was measured using a fabric air permeability tester (Wenzhou Darong Textile Instrument Co., Ltd., Model YG(B)461EC) in accordance with GB / T 5453-1997.

[0218] The moisture permeability of the polyimide nanofiber flakes of Examples 1 to 6 and Comparative Examples 1 to 4 was measured using a fabric moisture permeability meter (Wenzhou Darong Textile Instrument Co., Ltd., Model YG(B)216TC) in accordance with GB / T12704.2-2009.

[0219] The results are shown in Table 2 below.

[0220] Table 2: Air permeability and moisture permeability of polyimide nanofiber flakes

[0221]

[0222] It can be seen from Table 2 that, compared with Comparative Examples 1 to 4, the air permeability and moisture permeability of the polyimide nanofiber flakes of Examples 1 to 6 prepared by the method of the present invention are significantly greater, indicating that the comfort level is higher.

[0223] Experimental Example 4 Measurement of Compression Rate and Recovery Rate

[0224] The compression rate and recovery rate of the polyimide nanofiber flakes of Examples 1 to 6 and Comparative Examples 1 to 4 were measured according to the test method of Appendix A of FZ / T 64003-2021 Spray-bonded Cotton Flakes. The results are shown in Table 3 below.

[0225] Table 3: Compression rate and recovery rate of polyimide nanofiber flakes

[0226] Compression rate (%) Response rate (%) Example 1 82 92 Example 2 83 93 Example 3 81 91 Example 4 85 92 Example 5 86 93 Example 6 83 92 Comparative Example 1 12 8 Comparative Example 2 88 94 Comparative Example 3 1 2 Comparative Example 4 83 93

[0227] It can be seen from Table 3 that the compression rate and recovery rate of the polyimide nanofiber flakes of Examples 1 to 6 of the present invention are relatively high, and are suitable for the field of thermal insulation; while the compression rate and recovery rate of the polyimide nanofiber flakes of Comparative Examples 1 and 3 are significantly lower, and the fluffy structure is poor, and are not suitable for the field of thermal insulation materials.

[0228] The above embodiments are only used to help understand the method and core idea of ​​the present invention. It should be noted that, for those skilled in the art, several improvements and modifications can be made to the present invention without departing from the principles of the present invention, and these improvements and modifications also fall within the scope of protection of the present invention.

Claims

1. A method for preparing a polyimide nanofiber flake, the method comprising the following steps: (1) using diamine and dianhydride monomers to synthesize hot-melt polyamic acid spinning solution A; (2) using diamine and dianhydride monomers to synthesize a partially melted polyamic acid spinning solution B; (3) electrospinning the hot-melt polyamic acid spinning solution A and the partially meltable polyamic acid spinning solution B to form a polyamic acid layer A and a polyamic acid layer B, respectively, and stacking them to form a polyamic acid composite nanofiber membrane, wherein the polyamic acid composite nanofiber membrane comprises a stacked combination of the polyamic acid layer A, the polyamic acid layer B and the polyamic acid layer A; (4) placing the polyamic acid composite nanofiber membrane between two insulating fiber webs arranged horizontally and parallel to each other, allowing statically charged hot air to pass through the polyamic acid composite nanofiber membrane from the bottom to the top from below the two insulating fiber webs to loosen the polyamic acid composite nanofiber membrane, thereby obtaining fluffy polyamic acid nanofiber flakes; (5) subjecting the fluffy polyamic acid nanofiber flakes to thermal imidization treatment to obtain a polyimide nanofiber flake with a multilayer structure, The polyamic acid layer A is completely melted during the thermal imidization treatment. The polyamic acid layer B is partially melted during the thermal imidization treatment.

2. The method according to claim 1, wherein: In step (1), The diamine monomer is one or more of diaminodiphenyl ether diamine (ODA), all-meta-triphenyl diether diamine (1,3,3-APB), bisphenol A diamine (BAPP) and 4,4-diaminodiphenyl sulfone (DDS), The dianhydride monomer is one or more of biphenyl dianhydride (BPDA), triphenyl diether dianhydride (HQPDA), diphenyl ether dianhydride (ODPA), benzophenone dianhydride (BTDA), bisphenol A dianhydride (BPADA) and diphenyl sulfide dianhydride (TDPA).

3. The method according to claim 1, wherein: In step (2), The diamine monomer is a combination of a type I diamine monomer and a type II diamine monomer, The type I diamine monomer is one or more of diaminodiphenyl ether diamine (ODA), all-meta-triphenyl diether diamine (1,3,3-APB) and bisphenol A diamine (BAPP), The type II diamine monomer is one or more of p-phenylenediamine (PPD), biphenylenediamine (Bz) and 4,4-diamino-2,2-dimethylbiphenyl (DMB), The dianhydride monomer is a combination of a type I dianhydride monomer and a type II dianhydride monomer, The type I dianhydride monomer is one or more of triphenyl diether dianhydride (HQPDA), diphenyl ether dianhydride (ODPA), benzophenone dianhydride (BTDA) and bisphenol A dianhydride (BPADA), The type II dianhydride monomer is one or more of biphenyl dianhydride (BPDA) and terephthalic anhydride (PMDA).

4. The method according to claim 1, wherein: In step (3), the electrospinning is performed by using a plurality of electrospinning spinnerets, wherein the plurality of electrospinning spinnerets include a three-layer spinning spinneret group. The number of the upper layer spinning spinnerets is 1 to 3, the number of the bottom layer spinning spinnerets is 1 to 3, and the number of the middle layer spinning spinnerets is 3 to 20.

5. The method according to claim 1, wherein: In step (4), The two insulating fiber nets are both aramid fiber nets, and the mesh size is 2 to 5 cm. The distance between the two insulating fiber meshes is 5 to 30 mm. The statically charged hot air is hot air with positive or negative charges, and the hot air temperature is 80-150°C.

6. The method according to claim 1, wherein: In step (5), the temperature of the thermal imidization treatment is 300-450°C.

7. A polyimide nanofiber flake prepared by the method of claim 1, wherein the flake comprises a superimide layer A, a polyimide layer B and a polyimide layer A. in, The density of the flakes is less than 5 mg / cm 3 , air permeability is less than 10mm / s, moisture permeability is greater than 6000g / (m 2 ·24h), compression rate is greater than 80%, and recovery rate is greater than 90%. 8 . The flakes according to claim 7 , wherein the polyimide layer A is a film-like windproof layer, and the polyimide layer B is a fluffy thermal insulation layer.

9. The flakes according to claim 7, wherein the polyimide layer A is obtained by thermal imidization of hot-melt polyamic acid, and the fiber diameter is 100-500 nm. The thickness of the polyimide layer A is 1 to 100 μm. The pore size of the polyimide layer A is 0.5-2 μm.

10. The flakes according to claim 7, wherein the polyimide layer B is obtained by thermal imidization of partially molten polyamic acid, and the fiber diameter is 500-1500 nm. The thickness of the polyimide layer B is 1 to 20 mm. The pore size of the polyimide layer B is 3-10 μm.