Nonwoven fabric and use thereof, and method for producing nonwoven fabric
By using a specific range of thermoplastic resin fibers and fatty acid amides in spunbond nonwovens, combined with the composition of high and low melting point resins, the problems of spunbond nonwovens sliding and not feeling soft are solved, and the stability and softness of the nonwovens are achieved. Improved softness for high-performance hygienic materials.
Patent Information
- Application Number
- CN202280006256.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2021-06-30
- Filing Date
- 2022-06-30
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2042-06-30
AI Technical Summary
Existing spunbond nonwovens are prone to slipping during the product packaging process, resulting in distortion, and are not soft to the touch, making it difficult to meet the touch and softness requirements of hygienic materials.
Using fiber containing thermoplastic resin, the average single filament fineness is above 0.7dtex and below 4.0dtex, the fiber contains 0.01% to 1.5% fatty acid amide, the surface coverage is between 20% and 90%, combining high melting point and low melting point The fiber composition of thermoplastic resin is used to manufacture nonwoven fabrics through the spunbond method, controlling the crystallinity of the fiber and the transfer of fatty acid amide.
It effectively inhibits the sliding properties of non-woven fabrics and provides sufficient softness and hand feel. It is suitable for absorbent items such as sanitary materials and improves the stability and use experience of the product.
Smart Images

Figure BDA0004113737410000201
Abstract
Description
Technical Field
[0001] The present invention relates to a nonwoven fabric and a use thereof, and a method for producing the nonwoven fabric. Background Art
[0002] In recent years, higher performance has been required for absorbent articles such as sanitary materials represented by disposable diapers, sanitary napkins, incontinence pads, etc., and in particular, softer sheets are required for the surface layer of disposable diapers that contacts the skin, the back layer that is required to have a good touch, and the pleats that are prone to irritation to the skin.
[0003] For example, the softness of a sanitary sheet is particularly manifested by the bending softness and smoothness of the sheet. By taking both of these two elements of softness into consideration, a soft feel as a sanitary sheet can be felt.
[0004] As a nonwoven fabric suitable for absorbent articles, Patent Document 1 listed below describes a spunbonded nonwoven fabric made of a polyolefin resin containing a fatty acid amide as a lubricant.
[0005] Prior art literature
[0006] Patent Literature
[0007] Patent Document 1: Japanese Patent Application Publication No. 2002-69820 Summary of the invention
[0008] Problem that the invention aims to solve
[0009] However, the spunbonded nonwoven fabric described in Patent Document 1 has a problem that the lubricant transferred to the fiber surface causes the stacked products to slip and become deformed during the packaging process of products containing the nonwoven fabric (for example, sanitary materials).
[0010] In view of the above problems, one aspect of the present invention aims to provide a nonwoven fabric and its use, as well as a method for manufacturing the nonwoven fabric, which can suppress the sliding of nonwoven fabrics in the manufacturing process of products such as sanitary materials containing the nonwoven fabric and can feel sufficient softness when touched by human hands.
[0011] Solutions for solving problems
[0012] The present invention includes the following aspects.
[0013] [1] A nonwoven fabric comprising fibers containing a thermoplastic resin, wherein the average single fiber fineness of the fibers is from 0.7 dtex to 4.0 dtex, the fibers contain fatty acid amide in an amount from 0.01% by mass to 1.5% by mass relative to the total mass of the fibers, and the fatty acid amide coverage on the surface of the fibers is from 20% to 90%.
[0014] [2] The nonwoven fabric according to aspect 1 above, wherein the fibers contain the fatty acid amide in an amount of 0.6% by mass or less based on the total mass of the fibers.
[0015] [3] The nonwoven fabric according to aspect 1 or 2 above, wherein the fibers contain the fatty acid amide in an amount of 0.1% by mass or more relative to the total mass of the fibers.
[0016] [4] The nonwoven fabric according to any one of aspects 1 to 3, wherein the thermoplastic resin is a polyolefin, and the birefringence Δn of the fiber is 0.015 or more and 0.029 or less.
[0017] [5] The nonwoven fabric according to any one of aspects 1 to 4 above, wherein the fatty acid portion of the fatty acid amide has 22 or less carbon atoms.
[0018] [6] The nonwoven fabric according to any one of aspects 1 to 5 above, wherein the fatty acid amide is erucamide.
[0019] [7] A nonwoven fabric according to any one of the above-mentioned methods 1 to 6, wherein the above-mentioned thermoplastic resin contains 70% by mass or more and 99% by mass or less of a high-melting-point thermoplastic resin having a melting point higher than a predetermined melting point, and contains 1% by mass or more and 30% by mass or less of a low-melting-point thermoplastic resin having a melting point below the above-mentioned predetermined melting point.
[0020] [8] The nonwoven fabric according to any one of aspects 1 to 7 above, which is a long-fiber nonwoven fabric.
[0021] [9] An absorbent article comprising the nonwoven fabric according to any one of aspects 1 to 8 above.
[0022]
[10] The absorbent article according to aspect 9 above, which is a disposable diaper, a sanitary napkin or an incontinence pad.
[0023]
[11] A method for producing a nonwoven fabric, which is the method for producing a nonwoven fabric according to any one of the above aspects 1 to 8,
[0024] The above method is a spunbond method including a spinning step, a cooling step, a collecting step and a bonding step.
[0025] The ejection speed in the spinning step is 4 m / min or more and 8 m / min or less,
[0026] The cooling air velocity in the cooling step is 0.5 m / s or more and 1.5 m / s or less.
[0027]
[12] The method for producing a nonwoven fabric according to aspect 11 above, wherein the fatty acid amide is erucamide.
[0028] Effects of the Invention
[0029] The nonwoven fabric of one embodiment of the present invention suppresses the slippage of nonwoven fabrics in the production process of products such as sanitary materials including the nonwoven fabric, and has sufficient softness that can be felt when touched by human hands. DETAILED DESCRIPTION
[0030] Hereinafter, exemplary embodiments of the present invention (also referred to as present embodiments in this disclosure) will be described in detail, but the present invention is not limited to these embodiments.
[0031] The inventors of the present invention have conducted intensive research to solve the above-mentioned problems and have found that, for a nonwoven fabric formed from fibers containing a thermoplastic resin, the fibers have a specific average single fiber fineness, the fibers contain a specific amount of fatty acid amide, and the fatty acid amide coverage on the fiber surface is controlled within a specific range, thereby suppressing the slippage of the nonwoven fabrics and obtaining sufficient softness.
[0032] <Nonwoven fabrics>
[0033] One embodiment of the present invention provides a nonwoven fabric, which is a nonwoven fabric formed from fibers containing a thermoplastic resin, wherein the average single fiber fineness of the fibers is greater than or equal to 0.7 dtex and less than or equal to 4.0 dtex, the fibers contain fatty acid amide in an amount of greater than or equal to 0.01 mass % and less than or equal to 1.5 mass % relative to the total mass of the fibers, and the fatty acid amide coverage on the fiber surface is greater than or equal to 20% and less than or equal to 90%.
[0034] The nonwoven fabric of the present embodiment can be a long fiber nonwoven fabric manufactured by a spunbond method or a short fiber nonwoven fabric manufactured by a carding method, a wet papermaking method or the like. However, from the viewpoints of strength, productivity, and reduced irritation to the skin, a long fiber nonwoven fabric is preferred. In the present disclosure, a long fiber nonwoven fabric refers to a nonwoven fabric defined in JIS-L-0222. The fiber length of the long fiber can be, for example, 55 mm or more.
[0035] The nonwoven fabric of the present embodiment is composed of fibers containing thermoplastic resins. As thermoplastic resins, polyolefins such as polyethylene, polypropylene, or copolymers of ethylene and / or propylene with other olefins, polyesters such as polyethylene terephthalate, and polylactic acid can be listed. In addition, thermoplastic resins can be obtained by manufacturing petroleum as a raw material, or can be manufactured by biomass raw materials. Polypropylene can be a polymer synthesized by a conventional Ziegler-Natta catalyst, or a polymer synthesized by a single-site active catalyst represented by a metallocene. As other olefins, olefins with 4 to 10 carbon atoms, specifically 1-butene, 1-pentene, 1-hexene, 4-methyl-1-pentene, and 1-octene, etc. can be listed. These other olefins can be one alone or in combination of two or more. From the viewpoint of excellent dimensional stability during the production of products such as sanitary materials, it is preferred to use polypropylene-based fibers as fibers composed of polypropylene homopolymers and / or polypropylene copolymers.
[0036] In addition, the MFR (melt mass flow rate) of the thermoplastic resin is preferably 5 g / 10 minutes or more and 150 g / 10 minutes or less, more preferably 5 g / 10 minutes or more and 100 g / 10 minutes or less, further preferably 10 g / 10 minutes or more and 85 g / 10 minutes or less, particularly preferably 15 g / 10 minutes or more and 70 g / 10 minutes or less, and most preferably 20 g / 10 minutes or more and 65 g / 10 minutes or less. The MFR is determined by measuring in accordance with Table 1 of JIS-K7210 "Test methods for melt mass flow rate (MFR) and melt volume flow rate (MVR) of thermoplastics", at a test temperature of 230°C and a test load of 2.16 kg.
[0037] The thermoplastic resin constituting the fiber can be composed of two or more resins with different melting points. In one embodiment, the thermoplastic resin contains a high melting point thermoplastic resin having a melting point higher than a predetermined melting point, and a low melting point thermoplastic resin having a melting point below the predetermined melting point. The predetermined melting point is set as required. It should be noted that the melting point disclosed herein refers to the temperature corresponding to the maximum value of the endothermic peak when measured from 30°C to 300°C using a differential scanning calorimeter (DSC) at a heating rate of 10°C / min. Preferably, relative to the total mass of the thermoplastic resin 100% by mass, the content of the high melting point thermoplastic resin is 70% by mass or more and 99% by mass or less, and the content of the low melting point thermoplastic resin is 1% by mass or more and 30% by mass or less, and more preferably the content of the high melting point thermoplastic resin is 80% by mass or more and 97% by mass or less, and the content of the low melting point thermoplastic resin is 3% by mass or more and 20% by mass or less. When the content of the low melting point thermoplastic resin is within the above range, it is easy to manufacture a nonwoven fabric having good strength and good bending flexibility. The high melting point thermoplastic resin and the low melting point thermoplastic resin can be respectively composed of one or more resins, and each resin is classified as a high melting point thermoplastic resin or a low melting point thermoplastic resin according to whether its melting point exceeds a predetermined melting point or is below a predetermined melting point.
[0038] From the viewpoint of controlling the crystallinity of the fiber (more specifically, reducing the crystallinity) and inhibiting the transfer of fatty acid amide to the fiber surface, the difference between the melting point of the high-melting-point thermoplastic resin (the lowest melting point when there are two or more resins) and the melting point of the low-melting-point thermoplastic resin (the highest melting point when there are two or more resins) is preferably 10°C or more, or 20°C or more, or 30°C or more, and preferably 200°C or less, or 180°C or less, or 160°C or less.
[0039] The predetermined melting point can be set in a range of 80°C to 200°C in one embodiment, for example, 80°C, 85°C, 90°C, 95°C, 100°C, 105°C, 110°C, 115°C, 120°C, 130°C, 140°C, 150°C, 160°C, 170°C, 180°C, 190°C, or 200°C.
[0040] The melting point of the high melting point thermoplastic resin (when there are two or more resins, each melting point) is preferably higher than 80°C, 90°C or higher, or 100°C or higher, and is preferably 300°C or lower, 280°C or lower, or 260°C or lower.
[0041] The melting point of the low melting point thermoplastic resin (when there are two or more resins, each melting point) is preferably 40°C or higher, 50°C or higher, or 60°C or higher, and is preferably 200°C or lower, 180°C or lower, or 160°C or lower.
[0042] As the high melting point thermoplastic resin, resins such as the above-mentioned polyethylene, polypropylene, or copolymers of their monomers and other olefins can be exemplified. In addition, as the low melting point thermoplastic resin, it is preferably a resin having a melting point lower than that of the high melting point thermoplastic resin used by more than 10°C. The low melting point thermoplastic resin can be a random copolymer, an alternating copolymer, a block copolymer, or a graft copolymer. In addition, from the viewpoint of compatibility, it is preferred that the high melting point thermoplastic fiber and the low melting point thermoplastic resin both use the same monomer as the main component. For example, when the high melting point thermoplastic fiber is polypropylene, the low melting point thermoplastic resin is preferably a polypropylene resin (i.e., a homopolymer or copolymer of polypropylene). Furthermore, the low melting point thermoplastic resin can be a plastomer or an elastomer, without particular limitation.
[0043] The MFR of the high melting point thermoplastic resin is preferably 5 g / 10 minutes to 100 g / 10 minutes, more preferably 10 g / 10 minutes to 80 g / 10 minutes, further preferably 20 g / 10 minutes to 70 g / 10 minutes, and particularly preferably 30 g / 10 minutes to 60 g / 10 minutes. When the MFR is 5 g / 10 minutes to 100 g / 10 minutes, particularly 10 g / 10 minutes to 100 g / 10 minutes, yarn breakage is extremely rare, which is preferred from the viewpoint of spinnability.
[0044] The MFR of the low melting point thermoplastic resin is preferably 5 g / 10 minutes to 80 g / 10 minutes, more preferably 5 g / 10 minutes to 70 g / 10 minutes, further preferably 10 g / 10 minutes to 60 g / 10 minutes, and particularly preferably 10 g / 10 minutes to 40 g / 10 minutes. When the MFR is 5 g / 10 minutes to 80 g / 10 minutes, yarn breakage is very rare and spinnability is excellent.
[0045] The average single filament fineness of the fibers constituting the nonwoven fabric of the present embodiment is in one embodiment 0.7 dtex or more and 4.0 dtex or less, preferably 0.7 dtex or more and 3.0 dtex or less, more preferably 0.7 dtex or more and 2.0 dtex or less. The average single filament fineness is in one embodiment 0.7 dtex or more from the viewpoint of spinning stability, and in one embodiment 4.0 dtex or less from the viewpoint of imparting strength that is beneficial to sanitary materials (i.e., not too high) to the nonwoven fabric. It should be noted that there is a tendency that the thinner the average single filament fineness of the fibers constituting the nonwoven fabric, the softer it becomes.
[0046] When the thermoplastic resin contained in the fiber constituting the nonwoven fabric of the present embodiment contains a polyolefin or is a polyolefin, the birefringence Δn of the fiber is preferably 0.015 or more and 0.029 or less, more preferably 0.017 or more and 0.027 or less, further preferably 0.018 or more and 0.026 or less, and particularly preferably 0.019 or more and 0.025 or less. If the birefringence Δn is 0.015 or more and 0.029 or less, the crystallinity is low, so it is easy to control the amount of transfer of the fatty acid amide to the fiber surface. The method for measuring the birefringence Δn is described below.
[0047] The shape of the fibers constituting the nonwoven fabric of the present embodiment is not particularly limited, and may be core-sheath fibers, crimped fibers, etc. The cross-sectional shape of the single fiber may be a normal circular shape or a deformed cross-sectional shape.
[0048] The nonwoven fabric of the present embodiment contains fatty acid amide in an amount of 0.01 mass % or more and 1.5 mass % or less relative to the total mass of the fiber. From the viewpoint of the ease of transfer from the fiber to the fiber surface, that is, from the viewpoint of obtaining a good softness improvement effect using a relatively small amount of fatty acid amide, the fatty acid amide is preferably a fatty acid amide with a relatively low molecular weight, and the carbon number of the fatty acid part is preferably 24 or less, or 22 or less, or 20 or less. On the other hand, from the viewpoint of not making the transfer degree of fatty acid amide to the fiber surface too large and suppressing the sliding property of the nonwoven fabrics in the manufacturing process of the product containing the nonwoven fabric, the carbon number is preferably 12 or more, or 14 or more, or 16 or more, or 18 or more. As a specific example of suitable fatty acid amide, lauric acid amide, myristic acid amide, palmitic acid amide, stearic acid amide, behenic acid amide, oleic acid amide, erucic acid amide, etc. can be listed, and erucic acid amide is particularly preferred. These fatty acid amides can also be used in combination with a variety of them. Even if a relatively small amount of fatty acid amide is added, bending softness and ease of sliding can be significantly improved. If the content is too high, sliding is likely to occur in the manufacturing process of products (such as sanitary materials) containing nonwoven fabrics. Therefore, the content of fatty acid amide relative to the total mass of the fiber is suitable to be 1.5% by mass or less, in one embodiment, it is 0.01% by mass or more, preferably 0.1% by mass or more, more preferably 0.15% by mass or more, and particularly preferably 0.2% by mass or more. In addition, in one embodiment, it is 1.5% by mass or less, preferably 1.0% by mass or less, and particularly preferably 0.6% by mass or less.
[0049] The fatty acid amide coverage of the fiber surface constituting the nonwoven fabric of the present embodiment is 20% to 90%, preferably 25% to 80%, more preferably 30% to 70%. By making the fatty acid amide coverage of the fiber surface 20% to 90%, it is possible to achieve both the suppression of the sliding property of the nonwoven fabrics in the manufacturing process of the product containing the nonwoven fabric and sufficient softness. The method for measuring the fatty acid amide coverage of the fiber surface is described below.
[0050] In the nonwoven fabric of the present embodiment, the fibers may be joined by a partial thermocompression bonding (point bonding), a hot air method, a bonding method using a molten component (hot melt), and other various methods, and a partial thermocompression bonding method is preferred.
[0051] When the nonwoven fabric of the present embodiment is partially heat-pressed, the ratio of the area of the partially heat-pressed portion to the area of the nonwoven fabric (heat-pressed area ratio) is preferably 3% or more and 40% or less, more preferably 4% or more and 25% or less, particularly preferably 4% or more and 20% or less, and most preferably 5% or more and 15% or less from the viewpoint of strength retention and flexibility. In the present embodiment, the smaller the partial heat-pressed area ratio is, the easier it is to exert its softening effect. It should be noted that the partial heat-pressed area ratio is a value measured by a method of analyzing an image obtained by magnifying and photographing the nonwoven fabric using a microscope.
[0052] The nonwoven fabric of the present embodiment can have a concave-convex pattern formed by shaping in order to obtain good softness. As the concave-convex pattern, a straight line, a curve, an angle, a circle, a crepe structure, other continuous or discontinuous concave-convex patterns can be listed, and in order to improve the bending softness in the longitudinal direction (MD direction) and the transverse direction (CD direction), a tortoise shell pattern is preferably used. In addition, from the viewpoint of softness, the depth of the concave or convex portion (the maximum difference between the concave and the convex portion) is preferably 0.1 mm or more and 5.0 mm or less, more preferably 0.2 mm or more and 3.0 mm or less, and the greater the depth of the concave or convex portion, the greater the effect. In addition, in order to obtain good softness and touch, the area ratio of the concave-convex concave portion (pressing portion) relative to the nonwoven fabric area is preferably 5% or more and 40% or less, more preferably 5% or more and 25% or less. It should be noted that the maximum difference between the concave and the convex portion and the area ratio of the concave portion are values measured by a method of analyzing the image obtained by magnifying and photographing the nonwoven fabric using a microscope.
[0053] The nonwoven fabric of this embodiment preferably has a weight per unit area of 8 g / m 2 Above and 40g / m 2 Below, more preferably 10g / m 2 Above and 30g / m2 Below, particularly preferably 10g / m 2 Above and 25g / m 2 If the unit area weight is 8g / m 2 The above nonwoven fabric has good strength, especially suitable for sanitary materials. 2 The following nonwoven fabrics are preferred because they are excellent in softness and do not give a thick impression in appearance.
[0054] The nonwoven fabric of this embodiment may contain a hydrophilizing agent. As the hydrophilizing agent, it is preferred to use, in consideration of safety to the human body, safety during the process, etc., nonionic surfactants such as higher alcohols, higher fatty acids, alkylphenols, etc., to which ethylene oxide is added, anionic surfactants such as alkyl phosphates, alkyl sulfates, etc., alone or in the form of a mixture.
[0055] The content of the hydrophilizing agent varies depending on the performance required for the nonwoven fabric, and is generally preferably in the range of 0.1 to 1.0 parts by mass, more preferably 0.15 to 0.8 parts by mass, and further preferably 0.2 to 0.6 parts by mass, relative to 100 parts by mass of the fiber. If the content of the hydrophilizing agent is 0.1 to 1.0 parts by mass, the nonwoven fabric can have excellent hydrophilic properties and processability, particularly suitable for the surface layer of sanitary materials.
[0056] Furthermore, the nonwoven fabric of the present embodiment may contain a nucleating agent, a flame retardant, an inorganic filler, a pigment, a colorant, a heat stabilizer, an antistatic agent, and the like.
[0057] The nonwoven fabric of the present embodiment can achieve both reduced slipperiness and good softness by controlling the average single-filament fineness of the fibers and the presence of the fatty acid amide in the fibers and on the fiber surfaces.
[0058] In one mode, the sliding length of the nonwoven fabric is preferably below 40 mm, or below 35 mm, or below 30 m. If the sliding length is below 40 mm, it is not easy to slide in the manufacturing process of the product (such as sanitary material) containing the nonwoven fabric. The sliding length is considered from the viewpoint of the softness of the nonwoven fabric, and in one mode, it can be more than 8 mm, or more than 10 mm, or more than 12 mm. The measuring method of the sliding length is described below.
[0059] In one mode, the bending stiffness of the nonwoven fabric is preferably below 50 mm, or below 45 mm, or below 40 mm. If the bending stiffness is below 50 mm, the nonwoven fabric suitable for use as a sanitary material has a good feel. The bending stiffness is considered from the viewpoint of the ease of manufacture of the nonwoven fabric, and in one mode, it can be more than 10 mm, or more than 15 mm, or more than 20 mm. The determination method of the bending stiffness is described below.
[0060] The nonwoven fabric of the present embodiment can show good sealing performance by the coverage of the fatty acid amide on the fiber surface being within a specific range. In one embodiment, two nonwoven fabrics of the present embodiment are overlapped, and the peel strength of the sealed portion when laminating at a temperature of 150°C and a pressure of 1.4MPa can be preferably 0.5N / 5cm or more, or 0.7N / 5cm or more, or 1.0N / 5cm or more. If the above-mentioned peel strength is 0.5N / 5cm or more, a strength particularly suitable for absorbent articles can be obtained. From the perspective of the ease of manufacturing of the nonwoven fabric, the above-mentioned peel strength can be less than 25N / 5cm, or less than 23N / 5cm, or less than 21N / 5cm in one embodiment. The specific content of the method for measuring the peel strength is described below. One embodiment of the present invention also provides a nonwoven fabric having a sealing portion with a peel strength within the above-mentioned range. In addition, the sealing portion of the nonwoven fabric of the present embodiment can be formed by a joining method using a molten component (hot melt), a thermal bonding method, an ultrasonic method, or other various methods.
[0061] The tensile strength of the nonwoven fabric of the present embodiment is preferably 13N / 3cm or more, more preferably 13.5N / 3cm or more and 21N / 3cm or less, and further preferably 14N / 3cm or more and 20N / 3cm or less, as measured by the average value in the longitudinal and transverse directions. If the tensile strength is 13N / 3cm or more, the nonwoven fabric is not easy to break when used as a sanitary material, so it is preferred.
[0062] The stress at 5% elongation of the nonwoven fabric of the present embodiment is preferably 7N / 3cm or less, more preferably 3N / 3cm or more and 6.5N / 3cm or less, and further preferably 4N / 3cm or more and 6.5N / 3cm or less, as an average value of the longitudinal and transverse directions. If the stress at 5% elongation is 7N / 3cm or less, the nonwoven fabric has a good feel and excellent softness, especially as a sanitary material.
[0063] <Method for producing nonwoven fabric>
[0064] One embodiment of the present invention also provides a method for manufacturing a nonwoven fabric. The method for manufacturing the nonwoven fabric of the present embodiment is not particularly limited, and is preferably a spunbond method. The spunbond method generally includes a spinning process, a cooling process, a capturing process, and a bonding process. In the spinning process, the molten raw material resin is ejected from a nozzle. In the cooling process, the resin ejected through the spinning process is cooled by cold air to form a filament. In the capturing process, the filament is captured on a moving capturing surface to form a woven sheet. In the bonding process, the woven sheet is joined by partial hot pressing or the like. The spunbond method may have a stretching process between the cooling process and the capturing process in which the filament is stretched (pulled) using a high-speed airflow traction device using an air jet.
[0065] In the spinning process, the following formula is used:
[0066] Extrusion speed (m / min) = single hole extrusion volume (g / min) / {melt density (g / cm 3 )×[Single hole diameter (mm) / 2] 2 ×π}
[0067] The obtained ejection speed is preferably 1 m / min to 15 m / min, more preferably 3 m / min to 10 m / min, and particularly preferably 4 m / min to 8 m / min. If the ejection speed is 1 m / min or more, it is easy to suppress the excessive transfer of fatty acid amide to the fiber surface, and a nonwoven fabric having strength particularly advantageous for use as a sanitary material can be obtained, and if it is 15 m / min or less, no breakage or the like occurs, and stable spinning can be achieved.
[0068] In the spinning process, the temperature of the spinning spinneret is preferably 200°C to 300°C, more preferably 210°C to 280°C, and particularly preferably 220°C to 260°C. When the temperature of the spinning spinneret is set to 200°C to 300°C and spinning at a relatively low temperature, no excess heat is provided to the thermoplastic resin, so it is easy to suppress excessive transfer of fatty acid amide to the fiber surface. It should be noted that when a relatively high MFR (for example, an MFR of 5 g / 10 minutes or more at 230°C) is used as the thermoplastic resin, it is preferred because stable spinning can be performed even at a low spinning temperature.
[0069] In the cooling process, the cold air speed is preferably 0.4 m / s to 2.0 m / s, more preferably 0.5 m / s to 1.5 m / s. By setting the cold air speed to 0.4 m / s or more for rapid cooling, the crystallinity of the fiber is controlled (more specifically, the crystallinity is reduced), and the excessive transfer of fatty acid amide to the fiber surface is easily suppressed.
[0070] In the bonding process, it is preferred to integrate the front and back of the woven sheet captured by the capture process to the moving capture surface by joining. As a means of joining, partial hot pressing (point bonding) method, hot air method, joining method using molten components (hot melt), and other various methods can be listed, preferably partial hot pressing method. In the manufacture of the nonwoven fabric of this embodiment, partial hot pressing can be performed by ultrasonic method or through the woven sheet between heated embossing rollers, thereby integrating the front and back, such as dot-shaped pore shapes, elliptical shapes, diamond shapes, rectangular shapes, inclined broken white dot shapes and other sinking and floating patterns are scattered on the entire surface of the nonwoven fabric. Partial hot pressing is preferably performed using a heated embossing roller from the perspective of productivity. It should be noted that fatty acid amide and low-melting point thermoplastic resin also have the effect of reducing the pressing temperature of the nonwoven fabric, and can also alleviate the hardening phenomenon of the woven fabric caused by the filmization accompanying hot pressing. The method of making fatty acid amide and low-melting point thermoplastic resin contained in the fiber is preferably a polymer mixing method that is easy to evenly mix in the fiber.
[0071] When imparting a hydrophilizing agent to the nonwoven fabric of the present embodiment, as a method of imparting, a diluted hydrophilizing agent can usually be used, and existing methods such as dipping, spraying, coating (kiss coater, gravure roll coater, etc.) are adopted. It is preferred to dilute the hydrophilizing agent pre-mixed as needed with a solvent such as water for coating.
[0072] If the hydrophilizing agent is diluted with a solvent such as water and then applied, a drying step may be required. As a drying method at this time, a known method using convection heat transfer, heat conduction, radiation heat transfer, etc. can be used, and a drying method using hot air, infrared rays, or thermal contact can be used.
[0073] <Absorbent articles>
[0074] An absorbent article containing the above nonwoven fabric is also one aspect of the present invention. In one aspect, the absorbent article is a sanitary material for absorbing urine, scattered liquid, etc. The nonwoven fabric of the present invention has a good tactile feel and is therefore preferably used for an absorbent article worn by the human body. Specific examples of the absorbent article of the present invention include disposable diapers, sanitary napkins for physiological use, and incontinence pads.
[0075] Example
[0076] The present invention will be specifically described below by way of examples and comparative examples, but the present invention is not limited to the following examples. It should be noted that the evaluation methods of the various properties are as follows.
[0077] 1. Average single yarn fineness (dtex)
[0078] The nonwoven fabric was cut off from both ends of the nonwoven fabric in the width direction and divided into approximately five equal parts in the width direction. A 1 cm square test piece was sampled and the fiber diameter was measured at 20 points using an optical microscope (VHX-8000 manufactured by KEYENCE CORPORATION). The fineness was calculated from the average value.
[0079] 2. Weight per unit area (g / m 2 )
[0080] According to JIS-L1906, 5 test pieces of 20 cm in length and 5 cm in width are randomly collected from the nonwoven fabric, the weight is measured, and the average value is converted into the weight per unit area.
[0081] 3.MFR (g / 10 minutes)
[0082] The melt indexer (MELT INDEXER S-101 manufactured by Toyo Seiki Co., Ltd.) was used as a melt flow device to calculate the molten polymer discharge amount per 10 minutes from the time required to discharge a certain volume of thermoplastic resin under the conditions of an orifice diameter of 2.095 mm, an orifice length of 0.8 mm, a load of 2160 g, and a measuring temperature of 230°C.
[0083] 4. Melting point determination (DSC)
[0084] The measurement was performed using a differential scanning calorimeter (DSC) (manufactured by PerkinElmer Co., Ltd.: DSC6000). 3 mg of a thermoplastic resin was used as the measurement sample. The sample was spread over an aluminum open sample pan with a diameter of 5 mm, a clamping cover was placed, and the sample was fixed in the aluminum pan using a sample sealer. The temperature was increased from 30°C to 300°C in a nitrogen atmosphere at a heating rate of 10°C / min, and the maximum temperature of the melting endothermic curve was taken as the melting point.
[0085] 5. Spraying speed
[0086] The ejection speed is calculated by the following formula.
[0087] Extrusion speed (m / min) = single hole extrusion volume (g / min) / {melt density (g / cm 3 )×[Single hole diameter (mm) / 2] 2 ×π}
[0088] The melt density was calculated from the following formula using a melt indexer (MELT INDEXER S-101 manufactured by Toyo Seiki Co., Ltd.) or a melt flow rate device.
[0089] Melt density (g / cm 3 ) = weight of extrudate (g) / {cross-sectional area of flow hole (cm 2)×piston moving distance (cm)}
[0090] 6. Fatty acid amide coverage (%)
[0091] Ten fibers were collected from the nonwoven fabric, coated with osmium, and then morphologically observed using a field emission scanning electron microscope (FE-SEM) (manufactured by Hitachi High-Technologies Corporation: SU8220) at an accelerating voltage of 0.8 kV. The SEM image was binarized, and the area ratio of the attached matter on the fiber surface to the entire fiber was measured for each of the ten fibers, and the average of the ten fibers was calculated as the fatty acid amide coverage.
[0092] 7. Birefringence Δn
[0093] The birefringence of the nonwoven fabric was measured by the interference fringe method using a transmission quantitative interference microscope (Interphako, manufactured by Carl Zeiss Jena). The birefringence was measured at 10 points, and the average value of the birefringence at the 10 points was calculated as the birefringence Δn.
[0094] 8. Sliding length (mm) (sliding properties in the manufacturing process of sanitary materials)
[0095] A nonwoven fabric is pasted on the bottom of a weight of 20 cm in length, 10 cm in width, 2 cm in height, and 100 g in weight, which is assumed to be a sanitary material. The weight pasted with the nonwoven fabric is placed on other nonwoven fabrics pasted on a flat table in a manner that the nonwoven fabrics are in contact with each other, and the moving distance of the weight when a force of 3 N is applied to the side of the weight for 0.1 second is measured. The sliding length is calculated by the average value of each measured value of 5 points in the front and back and the longitudinal and transverse directions, a total of 20 points. The smaller the value of the sliding length (mm), the less likely it is to slip in the manufacturing process of the sanitary material.
[0096] 9. Bending stiffness (mm) (softness)
[0097] Measured according to the 45° cantilever method of JIS-L1096. Five test pieces with a width of 20 mm and a length of 150 mm are randomly collected from the nonwoven fabric sample in the longitudinal and transverse directions, and the short side of the test piece is placed on a smooth horizontal platform with a 45° inclined surface at one end, in accordance with the scale baseline. Then, the test piece is slowly slid in the direction of the inclined surface, and the position of the other end of the test piece when the center point of one end of the test piece contacts the inclined surface is measured using a scale. The length (mm) of the test piece movement is measured on the inside and outside of the five sheets, and these values are averaged as the bending stiffness.
[0098] 10. Seal peel strength (N / 5cm)
[0099] A test piece with a width of 5 cm and a length of 20 cm is randomly collected from the nonwoven fabric in the longitudinal and transverse directions. The embossed surfaces of the two collected nonwoven fabrics are overlapped with each other, and a heat sealer with a bonding width of 7 mm is used at a position 3 cm away from the end of one short side, and hot pressing is performed perpendicular to the length direction of the test piece and in the entire width area at a temperature of 150°C and a pressure of 1.4 MPa. A tensile testing machine is used to hold two nonwoven fabrics with a clamping interval of 5 cm in a manner in which the hot pressing part is the center, and a tensile test is performed by peeling the hot pressing part under the condition of a tensile speed of 30 cm / minute to determine the breaking strength. The sample is measured at 5 points in the longitudinal and transverse directions, and the measured values are averaged to calculate the breaking strength in the longitudinal direction and the breaking strength in the transverse direction, and these values are averaged as the peeling strength of the sealing part.
[0100] (Example 1)
[0101] To a polypropylene resin having an MFR of 55 g / 10 minutes (measured at a temperature of 230° C. and a load of 2.16 kg according to JIS-K7210) and a melting point of 160° C., erucic acid amide as a fatty acid amide in an amount of 0.4% by mass in the fiber and a polypropylene elastomer as a low melting point thermoplastic resin in an amount of 5% by mass in the fiber were added. The obtained mixture was extruded from a spinning nozzle having a nozzle diameter of 0.4 mm under the conditions of a single hole discharge amount of 0.5 g / min·hole, a spinning temperature of 230° C., and a discharge speed of 5.2 m / min, and the discharged yarn was cooled by cold air at a wind speed of 0.7 m / s, and then drawn by a high-speed airflow drawing device using an air jet, and captured on a moving collection surface to obtain a woven sheet. Next, the obtained woven sheet was passed between a smooth roller and an embossing roller (pattern specifications: diameter 0.5 mm, cross arrangement, horizontal spacing 2 mm, vertical spacing 2 mm, and pressing area ratio 6.3%), and the fibers were bonded to each other at a temperature of 136°C and a linear pressure of 35 kN / m to obtain a unit area weight of 15 g / m 2 The physical properties of the obtained long fiber nonwoven fabric are shown in Table 1.
[0102] (Example 2)
[0103] A long fiber nonwoven fabric was obtained in the same manner as in Example 1 except that the content of the fatty acid amide was 0.5 mass % and the content of the low melting point thermoplastic resin was 10 mass %.
[0104] (Example 3)
[0105] The content of the fatty acid amide was set to 0.7% by mass, the content of the low melting point thermoplastic resin was set to 0% by mass, and the weight per unit area was 17 g / m2 Except that the speed of the moving collection surface was adjusted in the manner of , a long-fiber nonwoven fabric was obtained in the same manner as in Example 1. The physical properties of the obtained long-fiber nonwoven fabric are shown in Table 1.
[0106] (Example 4)
[0107] A long-fiber nonwoven fabric was obtained in the same manner as in Example 3 except that the content of the fatty acid amide was 1.0% by mass. The physical properties of the obtained long-fiber nonwoven fabric are shown in Table 1.
[0108] (Example 5)
[0109] A long fiber nonwoven fabric was obtained in the same manner as in Example 1 except that a polypropylene resin having an MFR of 35 g / 10 minutes (measured at a temperature of 230° C. and a load of 2.16 kg according to JIS-K7210) was used, the content of the fatty acid amide was set to 0.8% by mass, the content of the low melting point thermoplastic resin was set to 4% by mass, and the spinning temperature was set to 250° C. The physical properties of the obtained long fiber nonwoven fabric are shown in Table 1.
[0110] (Example 6)
[0111] The content of the fatty acid amide was 0.3% by mass, the content of the low melting point thermoplastic resin was 3% by mass, and the weight per unit area was 17 g / m 2 The long-fiber nonwoven fabric was obtained in the same manner as in Example 5 except that the speed of the moving collection surface was adjusted in the manner of . The physical properties of the obtained long-fiber nonwoven fabric are shown in Table 1.
[0112] (Example 7)
[0113] A long fiber nonwoven fabric was obtained in the same manner as in Example 3 except that the content of the low melting point thermoplastic resin was changed to 2 mass %. The physical properties of the obtained long fiber nonwoven fabric are shown in Table 1.
[0114] (Example 8)
[0115] A long fiber nonwoven fabric was obtained in the same manner as in Example 3 except that the content of the fatty acid amide was 0.6% by mass and the content of the low melting point thermoplastic resin was 1% by mass. The physical properties of the obtained long fiber nonwoven fabric are shown in Table 1.
[0116] (Example 9)
[0117] A polyethylene resin having an MFR of 33 g / 10 minutes (measured at a temperature of 230° C. and a load of 2.16 kg according to JIS-K7210) and a melting point of 120° C. was used, the content of the fatty acid amide was set to 0.3% by mass, the content of the low-melting-point thermoplastic resin was set to 5% by mass, and the spinning temperature was set to 240° C., and a long fiber nonwoven fabric was obtained in the same manner as in Example 3. The physical properties of the obtained long fiber nonwoven fabric are shown in Table 1.
[0118] (Example 10)
[0119] As the core component, an extrudate of a mixture of a polypropylene resin having an MFR of 35 g / 10 min (measured at a temperature of 230° C. and a load of 2.16 kg according to JIS-K7210) and a melting point of 160° C., a fatty acid amide, and a low-melting thermoplastic resin was used, and as the sheath component, an extrudate of a mixture of a polyethylene resin having an MFR of 35 g / 10 min (measured at a temperature of 230° C. and a load of 2.16 kg according to JIS-K7210) and a melting point of 120° C., a fatty acid amide, and a low-melting thermoplastic resin was used to form a sheath-core structure with a ratio of 50 / 50 (mass ratio) of each component, and the content of the fatty acid amide was set to 0.4 mass % for both the sheath and core, the content of the low-melting thermoplastic resin was set to 5 mass % for both the sheath and core, and the spinning temperature was set to 240° C., and a long fiber nonwoven fabric was obtained in the same manner as in Example 3. The physical properties of the obtained long fiber nonwoven fabric are shown in Table 1.
[0120] (Example 11)
[0121] A long fiber nonwoven fabric was obtained in the same manner as in Example 3 except that the content of the fatty acid amide was 0.1% by mass and the content of the low melting point thermoplastic resin was 8% by mass. The physical properties of the obtained long fiber nonwoven fabric are shown in Table 1.
[0122] (Example 12)
[0123] A long fiber nonwoven fabric was obtained in the same manner as in Example 3 except that the content of the fatty acid amide was 0.2 mass % and the content of the low melting point thermoplastic resin was 15 mass %.
[0124] (Example 13)
[0125] A long-fiber nonwoven fabric was obtained in the same manner as in Example 1 except that the fatty acid amide was changed to stearic acid amide. The physical properties of the obtained long-fiber nonwoven fabric are shown in Table 1.
[0126] (Example 14)
[0127] A long-fiber nonwoven fabric was obtained in the same manner as in Example 1 except that the fatty acid amide was changed to oleic acid amide. The physical properties of the obtained long-fiber nonwoven fabric are shown in Table 1.
[0128] (Example 15)
[0129] A long-fiber nonwoven fabric was obtained in the same manner as in Example 1 except that the fatty acid amide was changed to ethylenebisstearic acid amide. The physical properties of the obtained long-fiber nonwoven fabric are shown in Table 1.
[0130] (Comparative Example 1)
[0131] A long fiber nonwoven fabric was obtained in the same manner as in Example 3 except that the content of the fatty acid amide was 0.005 mass % and the content of the low melting point thermoplastic resin was 5 mass %. The physical properties of the obtained long fiber nonwoven fabric are shown in Table 1.
[0132] (Comparative Example 2)
[0133] A long fiber nonwoven fabric was obtained in the same manner as in Example 3 except that the content of the fatty acid amide was 2.0 mass % and the content of the low melting point thermoplastic resin was 5 mass %. The physical properties of the obtained long fiber nonwoven fabric are shown in Table 1.
[0134] (Comparative Example 3)
[0135] A long fiber nonwoven fabric was obtained in the same manner as in Example 3 except that the content of the fatty acid amide was 0% by mass and the content of the low melting point thermoplastic resin was 5% by mass. The physical properties of the obtained long fiber nonwoven fabric are shown in Table 1.
[0136] (Comparative Example 4)
[0137] The content of fatty acid amide was set to 0.5 mass %, the content of low melting point thermoplastic resin was set to 10 mass %, and the fiber was extruded from a spinning nozzle with a nozzle diameter of 0.2 mm under the conditions of single hole discharge amount of 0.8 g / min·hole, spinning temperature of 250°C, and discharge speed of 33.6 m / min. The discharged fiber was cooled by cold air with a wind speed of 0.3 m / s, and the traction force of the air jet was set to 1.7 times. A long fiber nonwoven fabric was obtained in the same manner as in Example 3. The physical properties of the obtained long fiber nonwoven fabric are shown in Table 1.
[0138] (Comparative Example 5)
[0139] A long fiber nonwoven fabric was obtained in the same manner as in Example 1 except that the extrusion was carried out from a spinning nozzle having a nozzle diameter of 0.95 mm at a single hole discharge rate of 0.5 g / min·hole and a discharge speed of 0.9 m / min. The physical properties of the obtained long fiber nonwoven fabric are shown in Table 1.
[0140] (Comparative Example 6)
[0141] A long-fiber nonwoven fabric was obtained in the same manner as in Example 1 except that the fabric was cooled with cold air at a wind speed of 2.1 m / s. The physical properties of the obtained long-fiber nonwoven fabric are shown in Table 1.
[0142] [Table 1]
[0143]
[0144] Industrial Applicability
[0145] The nonwoven fabric provided by the present invention can be suitably used in absorbent articles such as sanitary materials, such as the surface layer, back layer, side pleats, etc. of disposable diapers, because it suppresses the sliding property of nonwoven fabrics in the manufacturing process of products (such as sanitary materials) containing the nonwoven fabrics and can feel sufficient softness when touched by human hands.
Claims
1. A nonwoven fabric comprising fibers containing a thermoplastic resin, wherein the average single filament fineness of the fibers is 0.7 dtex or more and 4.0 dtex or less, the fibers contain fatty acid amide in an amount of 0.01% by mass or more and 1.5% by mass or less relative to the total mass of the fibers, and the fatty acid amide coverage on the surface of the fibers is 20% or more and 90% or less, The thermoplastic resin is a polyolefin, the birefringence Δn of the fiber is greater than or equal to 0.015 and less than or equal to 0.029, The method for measuring the fatty acid amide coverage of the fiber surface is as follows: 10 fibers are collected from a nonwoven fabric, coated with osmium, and then morphologically observed using a field emission scanning electron microscope (FESEM) at an accelerating voltage of 0.8 kV. The SEM image is binarized, and for each of the 10 fibers, the area ratio of the attachments on the fiber surface to the entire fiber is measured, and the average of the 10 fibers is calculated as the fatty acid amide coverage.
2. The nonwoven fabric according to claim 1, wherein The fiber contains the fatty acid amide in an amount of 0.6 mass % or less based on the total mass of the fiber.
3. The nonwoven fabric according to claim 1 or 2, wherein: The fiber contains the fatty acid amide in an amount of 0.1 mass % or more based on the total mass of the fiber.
4. The nonwoven fabric according to claim 1 or 2, wherein: The fatty acid portion of the fatty acid amide has 22 or less carbon atoms.
5. The nonwoven fabric according to claim 1 or 2, wherein: The fatty acid amide is erucamide.
6. The nonwoven fabric according to claim 1 or 2, wherein: The thermoplastic resin contains 70% by mass or more and 99% by mass or less of a high melting point thermoplastic resin having a melting point higher than a predetermined melting point, and contains 1% by mass or more and 30% by mass or less of a low melting point thermoplastic resin having a melting point lower than the predetermined melting point. The predetermined melting point is 110°C, The high melting point thermoplastic resin is selected from the group consisting of polyethylene, polypropylene, or copolymers of these monomers and other olefins, and the low melting point thermoplastic resin is a resin having a melting point lower than that of the high melting point thermoplastic resin used by 10°C or more, and the high melting point thermoplastic resin and the low melting point thermoplastic resin are respectively composed of one or more resins. The nonwoven fabric according to claim 1 or 2, which is a long-fiber nonwoven fabric.