A method for preparing nitrogen-rich covalent triazine skeleton porous adsorption material
By simplifying the nucleophilic substitution reaction method, the nitrogen-rich covalent triazine skeleton porous materials were prepared, which solved the problems of long reaction time and high energy consumption, and achieved efficient adsorption performance, especially the adsorption performance of cationic dyes was significantly improved.
Patent Information
- Application Number
- CN202310392753.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-13
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2043-04-13
AI Technical Summary
The existing nucleophilic substitution reaction method has a long reaction time and high energy consumption, resulting in poor economicality and high carbonization of the material at high temperatures, which cannot accurately control the material structure, affecting the adsorption performance.
2,4,6-trichloro-1,3,5-triazine reacts with amino-containing monomers in an organic solvent, add catalyst and acid binding agent, wash and vacuum dry after condensation and reflux, shorten the reaction time and reduce the temperature and energy consumption, prepare nitrogen-rich covalent triazine skeleton porous adsorption materials.
The preparation of porous materials with simple operation, short time and low energy consumption is achieved, high temperature carbonization is avoided, and the adsorption performance on cationic dyes is significantly improved, and the adsorption capacity reaches 570mg/g.
Smart Images

Figure BDA0004176420040000031 
Figure BDA0004176420040000051 
Figure BDA0004176420040000061
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of porous adsorption material preparation, and in particular relates to a method for preparing a nitrogen-rich covalent triazine skeleton porous adsorption material. Background Art
[0002] With the rapid development of the printing and dyeing industry, the harmful wastewater generated has also increased. Dye wastewater has a large amount, complex composition, and is extremely difficult to degrade in the natural environment. If it is not treated, it will cause the ecological balance of the water to be destroyed, posing a great threat to the health of humans and other organisms. Therefore, economical and efficient treatment of dye wastewater is an important part of ensuring the sustainable development of the printing and dyeing industry. The methods for treating printing and dyeing wastewater include coagulation sedimentation, biological treatment, adsorption, ion exchange, etc. Among them, the adsorption method has been widely concerned due to its advantages of high removal efficiency, low cost and simple operation. The development of porous adsorbents with simple preparation, low cost, high adsorption capacity and high stability is one of the important research directions for solving dye wastewater pollution (Schwarzenbach RP, Escher BI, Fenner K., Hofstetter TB, Johnson CA, Gunten U.V., Wehrli B. The challenge of micropollutants in aquatic systems, Science, 2006, 313, 1072).
[0003] In recent years, organic porous polymer materials have gradually become a hot topic in porous material research. Compared with traditional porous materials (such as inorganic molecular sieves and inorganic-organic hybrid framework materials), organic porous polymers are generally composed of light elements such as carbon, hydrogen, oxygen, nitrogen and boron, and have the advantages of light framework density, large specific surface area and high physical and chemical stability. At the same time, the structure, properties and functions of organic porous polymers can be adjusted by selecting appropriate structural units, different types of functional groups and synthetic pathways. Based on the above advantages, organic porous polymer materials have shown application prospects in catalysis, gas storage, separation, environment, energy and other fields (Ren Hao, Zhu Guangshan. Organic Porous Materials: Synthesis Strategies and Properties, Acta Chemica Sinica, 2015, 73, 587; Wang H., Jiang D., Huang D., Zeng G., Xu P., Lai C., Chen M., Cheng M., Zhang C., Wang Z. Covalent triazine frameworks for carbon dioxide capture, Journal of Materials Chemistry A, 2019, 7, 22848).
[0004] Among the many types of organic porous polymers, covalent triazine frameworks (CTFs) contain aromatic 1,3,5-triazine rings in their structures. On the one hand, the triazine rings give CTFs abundant nitrogen sites. On the other hand, the conjugation between the triazine rings and the aromatic rings leads to a decrease in the energy of the overall structure of CTFs, which improves the chemical stability of CTFs. At present, researchers have developed a variety of methods for preparing CTFs, such as ZnCl2 ion thermal method, Friedel-Crafts reaction method, nucleophilic substitution reaction method, etc. (Krishnaraj C., Jena HS, Leus K., Van der Voort P. Covalent triazine frameworks-asustainable perspective, Green Chemistry, 2020, 22, 1038). Among them, the ion thermal method is cumbersome to operate, with high reaction temperature and long reaction time, which causes carbonization of porous materials; the substitution selectivity of electron-rich aromatic monomer sites in the Friedel-Crafts reaction method is not unique, so the structure of the material cannot be accurately determined; the nucleophilic substitution reaction method is simple to operate and the raw materials are cheap, which has attracted the attention of researchers. However, the current reaction time for preparing CTFs by the nucleophilic substitution reaction method is generally around 24h, with long reaction time, high energy consumption and poor economy. Therefore, for the nucleophilic substitution reaction method, it is of great significance to develop a simple and time-consuming reaction path for the synthesis of CTFs (Wang T., Kailasam K., Xiao P., Chen G., Chen L., Wang L., Li J., Zhu J. Adsorption removal of organic dyes on covalent triazine framework (CTF), Microporous and Mesoporous Materials, 2014, 187, 63). Summary of the invention
[0005] The object of the present invention is to provide a method for preparing a nitrogen-rich covalent triazine skeleton porous adsorption material, which can simplify the operation, shorten the reaction time, reduce the reaction temperature and energy consumption, thereby avoiding high-temperature carbonization of the porous material; the porous adsorption material obtained by the preparation method can greatly improve the adsorption performance of cationic dyes.
[0006] To achieve the above object, the present invention discloses a method for preparing a nitrogen-rich covalent triazine skeleton porous adsorption material, comprising the following steps:
[0007] (1) adding 2,4,6-trichloro-1,3,5-triazine and an amino-containing monomer into a reaction vessel containing an organic solvent, then adding a catalyst and an acid binding agent, and condensing and refluxing at 100-150° C. for 3-6 hours to obtain a crude product;
[0008] (2) washing the crude product with a solvent and filtering it to obtain a pure product;
[0009] (3) Drying the purified product under vacuum conditions to obtain a nitrogen-rich covalent triazine skeleton porous adsorption material.
[0010] Preferably, in step (1), the molar ratio of the amino monomer to 2,4,6-trichloro-1,3,5-triazine is (1.32-1.67):1; the molar ratio of the catalyst to 2,4,6-trichloro-1,3,5-triazine is (0.03-0.15):1; and the molar ratio of the acid binding agent to 2,4,6-trichloro-1,3,5-triazine is (3.3-8):1.
[0011] Preferably, in step (1), the molar ratio of the amino monomer to 2,4,6-trichloro-1,3,5-triazine is 1.5:1; the molar ratio of the catalyst to 2,4,6-trichloro-1,3,5-triazine is 0.09:1; and the molar ratio of the acid binding agent to 2,4,6-trichloro-1,3,5-triazine is 6:1.
[0012] Preferably, in step (1), the amino monomer is one of 1,3-diaminourea, p-phenylenediamine, 1,3-diaminoacetone and ethylenediamine.
[0013] Preferably, in step (1), the catalyst is potassium iodide or sodium iodide; and the acid binding agent is potassium carbonate or sodium carbonate.
[0014] Preferably, in step (1), the organic solvent is one of 1,4-dioxane, N,N-dimethylformamide, tetrahydrofuran and pyridine.
[0015] Preferably, in step (1), when the organic solvent is one of 1,4-dioxane, tetrahydrofuran and pyridine, the reaction temperature is 100°C; when the organic solvent is N,N-dimethylformamide, the reaction temperature is 150°C.
[0016] Preferably, in step (1), the concentration of 2,4,6-trichloro-1,3,5-triazine in the organic solvent is 0.06 mol / L.
[0017] Preferably, in step (2), the crude product is washed three times with three or four of deionized water, N,N-dimethylformamide, tetrahydrofuran and acetone respectively, and then filtered to obtain a pure product.
[0018] Preferably, in step (3), the pure product is heated to 100° C. under vacuum conditions and dried for 10 h.
[0019] Compared with the prior art, the present invention has the following advantages:
[0020] (1) The reaction of the present invention is carried out under normal pressure, the operation is simple, the reaction time is short, the reaction temperature is low, the energy consumption is low, and the overall reaction conditions are mild, thereby avoiding high-temperature carbonization of the porous material;
[0021] (2) The nitrogen-rich covalent triazine skeleton porous material prepared by the present invention has excellent adsorption performance for cationic dyes. DETAILED DESCRIPTION
[0022] The present invention is further described in detail below with reference to the embodiments.
[0023] Embodiment 1
[0024] 2,4,6-trichloro-1,3,5-triazine (TCT, 557.3 mg, 3.0 mmol) and 1,3-diaminourea (CHZ, 406.4 mg, 4.5 mmol) were added to a round-bottom flask containing a solvent of 1,4-dioxane (50 mL), and then catalyst KI (15.4 mg, 0.09 mmol) and acid-binding agent potassium carbonate (2484.9 mg, 18 mmol) were added, and the mixture was condensed and refluxed at 100°C for 4 h to obtain a crude product; the obtained mixture was filtered, and the filter cake was washed three times with deionized water, N,N-dimethylformamide (DMF), and tetrahydrofuran (THF) in turn, and the product was filtered; the obtained filter cake was heated to 100°C under vacuum conditions and dried for 10 h to obtain a yellowish brown powder CTF with a yield of 46%. According to infrared spectrum analysis, at about 850 cm -1 The C-Cl bond disappears, indicating the successful synthesis of the porous material. The reaction formula is as follows:
[0025]
[0026] Embodiment 2
[0027] 2,4,6-trichloro-1,3,5-triazine (TCT, 557.1 mg, 3.0 mmol) and 1,3-diaminourea (CHZ, 406.2 mg, 4.5 mmol) were added to a round-bottom flask containing a solvent of 1,4-dioxane (50 mL), and then catalyst KI (46.7 mg, 0.27 mmol) and acid-binding agent potassium carbonate (2483.0 mg, 18 mmol) were added, and the mixture was condensed and refluxed at 100°C for 4 h to obtain a crude product; the obtained mixture was filtered, and the filter cake was washed three times with deionized water, N,N-dimethylformamide (DMF), and acetone in turn, and the product was filtered; the obtained filter cake was heated to 100°C under vacuum conditions and dried for 10 h to obtain a yellowish brown powder CTF with a yield of 50%. According to infrared spectrum analysis, at about 850 cm -1 The C-Cl bond disappears, indicating the successful synthesis of the porous material. The reaction formula is the same as that of Example 1.
[0028] Embodiment 3
[0029] 2,4,6-trichloro-1,3,5-triazine (TCT, 555.8 mg, 3.0 mmol) and 1,3-diaminourea (CHZ, 406.3 mg, 4.5 mmol) were added to a round-bottom flask containing a solvent of 1,4-dioxane (50 mL), and then catalyst KI (76.9 mg, 0.45 mmol) and acid-binding agent potassium carbonate (2485.5 mg, 18 mmol) were added, and the mixture was condensed and refluxed at 100°C for 4 h to obtain a crude product; the obtained mixture was filtered, and the filter cake was washed three times with deionized water, N,N-dimethylformamide (DMF), and tetrahydrofuran (THF) in turn, and the product was filtered; the obtained filter cake was heated to 100°C under vacuum conditions and dried for 10 h to obtain a yellowish brown powder CTF with a yield of 33%. According to infrared spectrum analysis, at about 850 cm -1 The C-Cl bond disappears, indicating the successful synthesis of the porous material. The reaction formula is the same as that of Example 1.
[0030] Embodiment 4
[0031] 2,4,6-trichloro-1,3,5-triazine (TCT, 553.2 mg, 3.0 mmol) and 1,3-diaminourea (CHZ, 405.4 mg, 4.5 mmol) were added to a round-bottom flask containing a solvent of 1,4-dioxane (50 mL), and then catalyst KI (46.7 mg, 0.27 mmol) and acid-binding agent potassium carbonate (2484.9 mg, 18 mmol) were added, and the mixture was condensed and refluxed at 100°C for 3 h to obtain a crude product; the obtained mixture was filtered, and the filter cake was washed three times with deionized water, N,N-dimethylformamide (DMF), and tetrahydrofuran (THF) in turn, and the product was filtered; the obtained filter cake was heated to 100°C under vacuum conditions and dried for 10 h to obtain a yellowish brown powder CTF with a yield of 37%. According to infrared spectrum analysis, at about 850 cm -1 The C-Cl bond disappears, indicating the successful synthesis of the porous material. The reaction formula is the same as that of Example 1.
[0032] Embodiment 5
[0033] 2,4,6-trichloro-1,3,5-triazine (TCT, 557.3 mg, 3.0 mmol) and 1,3-diaminourea (CHZ, 406.4 mg, 4.5 mmol) were added to a round-bottom flask containing a solvent of 1,4-dioxane (50 mL), and then catalyst KI (46.7 mg, 0.27 mmol) and acid-binding agent sodium carbonate (1090 mg, 10.3 mmol) were added, and the mixture was condensed and refluxed at 100°C for 4 h to obtain a crude product; the obtained mixture was filtered, and the filter cake was washed three times with deionized water, N,N-dimethylformamide (DMF), and acetone in turn, and the product was filtered; the obtained filter cake was heated to 100°C under vacuum conditions and dried for 10 h to obtain a yellowish brown powder CTF with a yield of 80%. According to infrared spectrum analysis, at about 850 cm -1 The C-Cl bond disappears, indicating the successful synthesis of the porous material. The reaction formula is the same as that of Example 1.
[0034] Embodiment 6
[0035] 2,4,6-trichloro-1,3,5-triazine (TCT, 557.2 mg, 3.0 mmol) and 1,3-diaminourea (CHZ, 405.4 mg, 4.5 mmol) were added to a round-bottom flask containing solvent N,N-dimethylformamide (DMF, 50 mL), and then catalyst KI (46.7 mg, 0.27 mmol) and acid-binding agent potassium carbonate (2484.9 mg, 18 mmol) were added, and the crude product was obtained by condensation and reflux at 150°C for 4 h; the obtained mixture was filtered, and the filter cake was washed three times with deionized water, N,N-dimethylformamide (DMF), tetrahydrofuran (THF), and acetone in turn, and the product was filtered; the obtained filter cake was heated to 100°C under vacuum conditions and dried for 10 h to obtain a yellowish brown powder CTF with a yield of 40%. According to infrared spectrum analysis, at about 850 cm -1 The C-Cl bond disappears, indicating the successful synthesis of the porous material. The reaction formula is the same as that of Example 1.
[0036] Embodiment 7
[0037] 2,4,6-trichloro-1,3,5-triazine (TCT, 553.2 mg, 3.0 mmol) and 1,3-diaminourea (CHZ, 405.4 mg, 4.5 mmol) were added to a round-bottom flask containing a solvent of pyridine (50 mL), and then catalyst KI (46.7 mg, 0.27 mmol) and acid-binding agent potassium carbonate (2484.9 mg, 18 mmol) were added, and the mixture was condensed and refluxed at 100°C for 4 h to obtain a crude product; the obtained mixture was filtered, and the filter cake was washed three times with ultrapure water, N,N-dimethylformamide (DMF), and tetrahydrofuran (THF) in turn, and the product was filtered; the obtained filter cake was heated to 100°C under vacuum conditions and dried for 10 h to obtain a yellowish brown powder CTF with a yield of 45%. According to infrared spectrum analysis, at about 850 cm -1 The C-Cl bond disappears, indicating the successful synthesis of the porous material. The reaction formula is the same as that of Example 1.
[0038] Embodiment 8
[0039] 2,4,6-trichloro-1,3,5-triazine (TCT, 557.3 mg, 3.0 mmol) and 1,3-diaminourea (CHZ, 406.4 mg, 4.5 mmol) were added to a round-bottom flask containing a solvent of tetrahydrofuran (THF, 50 mL), and then a catalyst of NaI (40.5 mg, 0.27 mmol) and an acid-binding agent of sodium carbonate (1907.8 mg, 18 mmol) were added, and the mixture was condensed and refluxed at 100°C for 6 h to obtain a crude product; the obtained mixture was filtered, and the filter cake was washed three times with deionized water, N,N-dimethylformamide (DMF), and tetrahydrofuran (THF) in turn, and the product was filtered; the obtained filter cake was heated to 100°C under vacuum conditions and dried for 10 h to obtain a yellowish brown powder CTF with a yield of 44%. According to infrared spectrum analysis, at about 850 cm -1 The C-Cl bond disappears, indicating the successful synthesis of the porous material. The reaction formula is as follows:
[0040]
[0041] Embodiment 9
[0042] 2,4,6-trichloro-1,3,5-triazine (TCT, 557.3 mg, 3.0 mmol) and p-phenylenediamine (PD, 486.63 mg, 4.5 mmol) were added to a round-bottom flask containing a solvent of 1,4-dioxane (50 mL), and then catalyst KI (44.8 mg, 0.27 mmol) and acid-binding agent potassium carbonate (2484.9 mg, 18 mmol) were added, and the mixture was condensed and refluxed at 100°C for 4 h to obtain a crude product; the obtained mixture was filtered, and the filter cake was washed three times with deionized water, N,N-dimethylformamide (DMF), tetrahydrofuran (THF), and acetone in turn, and the product was filtered; the obtained filter cake was heated to 100°C under vacuum conditions and dried for 10 h to obtain powdered CTF with a yield of 56%. According to infrared spectrum analysis, at about 850 cm -1 The C-Cl bond disappears, indicating the successful synthesis of the porous material. The reaction formula is as follows:
[0043]
[0044] Embodiment 10
[0045] 2,4,6-trichloro-1,3,5-triazine (TCT, 557.3 mg, 3.0 mmol) and 1,3-diaminoacetone (DAP, 378.25 mg, 4.5 mmol) were added to a round-bottom flask containing a solvent of 1,4-dioxane (50 mL), and then catalyst KI (45.4 mg, 0.27 mmol) and acid-binding agent potassium carbonate (2484.9 mg, 18 mmol) were added, and the mixture was condensed and refluxed at 100°C for 6 h to obtain a crude product; the obtained mixture was filtered, and the filter cake was washed three times with deionized water, N,N-dimethylformamide (DMF), and tetrahydrofuran (THF) in turn, and the product was filtered; the obtained filter cake was heated to 100°C under vacuum conditions and dried for 10 h to obtain powdered CTF with a yield of 58%. According to infrared spectrum analysis, at about 850 cm -1 The C-Cl bond disappears, indicating the successful synthesis of the porous material. The reaction formula is as follows:
[0046]
[0047] Embodiment 11
[0048] 2,4,6-trichloro-1,3,5-triazine (TCT, 557.3 mg, 3.0 mmol) and ethylenediamine (en, 90.34 mg, 4.5 mmol) were added to a round-bottom flask containing solvent 1,4-dioxane (50 mL), and then catalyst KI (44.3 mg, 0.27 mmol) and acid-binding agent potassium carbonate (2484.9 mg, 18 mmol) were added, and the mixture was condensed and refluxed at 100°C for 4 h to obtain a crude product; the obtained mixture was filtered, and the filter cake was washed three times with deionized water, N,N-dimethylformamide (DMF), tetrahydrofuran (THF), and acetone in turn, and the product was filtered; the obtained filter cake was heated to 100°C under vacuum conditions and dried for 10 h to obtain powdered CTF with a yield of 48%. According to infrared spectrum analysis, at about 850 cm -1 The C-Cl bond disappears, indicating the successful synthesis of the porous material. The reaction formula is as follows:
[0049]
[0050] 5 mg of the nitrogen-rich CTFs samples prepared in Examples 1 to 11 were added to 10 mL of methylene blue (MB) solutions of different concentrations, and adsorbed at 303 K for 24 h under constant temperature oscillation. After the adsorption, the residual concentration of MB was measured by ultraviolet spectrophotometer, and then the adsorption capacity of MB was determined by analysis, and the results are shown in Table 1.
[0051] Table 1 Adsorption capacity of nitrogen-rich CTFs samples for MB
[0052]
[0053] As shown in Table 1, the MB adsorption capacity of the nitrogen-rich CTFs samples prepared in the above examples is affected by the reaction monomer structure, reaction solvent, reaction temperature, reaction time, types of catalyst and acid-binding agent, and catalyst equivalent ratio during the CTFs preparation process. The maximum MB adsorption capacity of nitrogen-rich CTFs is 570 mg / g, showing a high dye removal effect.
Claims
1. A method for preparing a nitrogen-rich covalent triazine framework porous adsorption material, characterized in that: The following steps are involved: (1) adding 2,4,6-trichloro-1,3,5-triazine and an amino-containing monomer into a reaction vessel containing an organic solvent, then adding a catalyst and an acid binding agent, and condensing and refluxing at 100-150° C. for 3-6 hours to obtain a crude product; The catalyst is potassium iodide or sodium iodide; the amino monomer is 1,3-diaminourea or 1,3-diaminoacetone; The molar ratio of the amino monomer to 2,4,6-trichloro-1,3,5-triazine is (1.32-1.67):1; the molar ratio of the catalyst to 2,4,6-trichloro-1,3,5-triazine is (0.03-0.15):1; the molar ratio of the acid binding agent to 2,4,6-trichloro-1,3,5-triazine is (3.3-8):1; The organic solvent is one of 1,4-dioxane, N,N-dimethylformamide, tetrahydrofuran and pyridine; (2) washing the crude product with a solvent and filtering it to obtain a pure product; (3) Drying the purified product under vacuum conditions to obtain a nitrogen-rich covalent triazine skeleton porous adsorption material.
2. The method for preparing a nitrogen-rich covalent triazine framework porous adsorption material according to claim 1, characterized in that: In step (1), the molar ratio of the amino monomer to 2,4,6-trichloro-1,3,5-triazine is 1.5:1; the molar ratio of the catalyst to 2,4,6-trichloro-1,3,5-triazine is 0.09:1; and the molar ratio of the acid binding agent to 2,4,6-trichloro-1,3,5-triazine is 6:
1.
3. The method for preparing a nitrogen-rich covalent triazine framework porous adsorption material according to claim 1 or 2, characterized in that: In step (1), the acid binding agent is potassium carbonate or sodium carbonate.
4. The method for preparing a nitrogen-rich covalent triazine framework porous adsorption material according to claim 1, characterized in that: In step (1), when the organic solvent is one of 1,4-dioxane, tetrahydrofuran and pyridine, the reaction temperature is 100°C; when the organic solvent is N,N-dimethylformamide, the reaction temperature is 150°C.
5. The method for preparing a nitrogen-rich covalent triazine framework porous adsorption material according to claim 1, characterized in that: In step (1), the concentration of 2,4,6-trichloro-1,3,5-triazine in the organic solvent is 0.06 mol / L.
6. The method for preparing a nitrogen-rich covalent triazine framework porous adsorption material according to claim 1, characterized in that: In step (2), the crude product is washed three times with three or four of deionized water, N,N-dimethylformamide, tetrahydrofuran and acetone respectively, and then filtered to obtain a pure product.
7. The method for preparing a nitrogen-rich covalent triazine framework porous adsorption material according to claim 1, characterized in that: In step (3), the purified product is heated to 100° C. under vacuum conditions and dried for 10 h.
Citation Information
Patent Citations
Amino end-group triazine ring tree-shaped macromolecular adsorbent and preparation method thereof
CN102600809A
Preparation method and application of nitrogen-rich adsorbent for removing perfluorinated and polyfluorinated alkyl substances (PFAS) from water
CN115739047A