A method for preparing a solid superbase and using it to catalyze the degradation of waste polycarbonate
Patent Information
- Application Number
- CN202310015523.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-01-04
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2043-01-04
AI Technical Summary
Existing alkali catalysts are difficult to reuse in the chemical degradation of spent polycarbonate, and residues in the product may affect further application.
The solid super-strong alkali catalyst K2O/SnO2-ZrO2 is used to catalyze the degradation of waste polycarbonate by preparation method, to form bisphenol compounds and carbonate compounds, and to achieve reusing of the catalyst through post-treatment.
It has achieved efficient degradation of waste polycarbonate, the catalyst can be reused for more than 10 times, and its performance is still excellent, solving the problem that traditional homogeneous alkaline catalysts cannot be reused, and promoting the resource utilization of waste plastics.
Smart Images

Figure BDA0004037108330000051 
Figure BDA0004037108330000061 
Figure BDA0004037108330000062
Abstract
Description
Technical Field
[0001] The invention belongs to the field of chemical recycling of waste plastics, and specifically relates to use of a solid superbase in catalytic degradation of waste polycarbonate, and a method for catalytic degradation of waste polycarbonate by the solid superbase to generate bisphenol compounds and carbonate. Technical Background
[0002] Polycarbonate, also known as PC, has excellent mechanical properties, heat aging resistance, chemical corrosion resistance and other properties. It is widely used in optics, automobiles, electronic appliances, packaging, health care and other fields. It is the fastest growing general engineering plastic among the five major engineering plastics. Its preparation methods mainly include ester exchange method and phosgene method. At present, there is an annual production capacity of about 2.5 million tons in China alone. At the same time, more and more waste polycarbonate materials are generated. Although waste polycarbonate itself is less toxic, it is difficult to degrade under natural conditions. The usual landfill or incineration treatment either occupies a large amount of land resources or produces waste gas to pollute the environment. The recycling of PC is increasingly valued by the industry.
[0003] Generally, there are two methods for recycling PC: physical method and chemical method. The former is to re-prepare PC products by melt remolding or granulation remolding, but it is generally downgraded and the product value is reduced; the latter is to degrade PC into monomers or products by chemical degradation, thereby realizing the recycling of waste PC. Predecessors have done a lot of work on PC degradation. For example, Pan Zhiyan and others from Zhejiang University of Technology have successively studied the degradation behavior of PC in supercritical / subcritical ethanol, toluene, water and other media. PC can be almost completely degraded into bisphenol A. Patent CN 101407450A uses easily recyclable solvents, conventional inorganic bases or their complexes to achieve a PC degradation rate of more than 98% under relatively mild reaction conditions. SABIC discloses a method for preparing dihydroxy aromatic compounds by alcoholysis of a composition containing polycarbonate in patent CN104718238B. The catalysts used are mainly hydroxides, hydrides, organic salts, oxides, etc. of alkali metals, alkaline earth metals, and some transition metals. The product after PC degradation is refined to obtain bisphenol A products. Patent CN 101429100B uses ionic liquids such as 1-allyl-3-methylimidazole chloride and 1-butyl-3-methylimidazole bromide as reaction media and catalysts to achieve chemical degradation of PC. After the reaction is completed, ethyl acetate is added, and the upper layer is distilled to obtain a bisphenol A product, and the ionic liquid in the lower layer is reused as a reaction medium and catalyst; Patent CN 113527096 A adds microwave to the conventional base-catalyzed alcoholysis of PC to strengthen the process, which can shorten the degradation time and achieve selective degradation of PC without transition metal base catalysis.
[0004] It is not difficult to see from the above process that the base-catalyzed alcoholysis process can achieve the chemical degradation of PC, but since most of the catalysts are homogeneous alkaline catalysts, additional operations are required for separation from the product, and it is difficult to achieve reuse. Summary of the invention
[0005] The purpose of the present invention is to solve the above technical problems and provide a method for catalyzing the degradation of waste polycarbonate to generate bisphenol compounds and carbonate compounds by solid superbase. The catalyst preparation method is simple and low in cost. After being reused for more than 10 times, its catalytic performance is still excellent. The problem that traditional homogeneous alkaline catalysts cannot be reused and the residue in the product may affect the further application of the product is solved.
[0006] Another object of the present invention is to provide a use of a solid superbase in catalytic degradation of waste polycarbonate, which can degrade waste polycarbonate into bisphenol compounds and carbonate compounds, thereby realizing resource utilization of waste plastics.
[0007] To achieve the above-mentioned object of the invention, the technical solution of the present invention is as follows:
[0008] A method for catalyzing the degradation of waste polycarbonate using a solid superbase comprises preparing a mixed solution of waste polycarbonate, alcohol, solvent and catalyst, heating the solution for reaction, completely degrading the waste polycarbonate into bisphenol compounds and carbonate compounds, and obtaining a product after post-treatment. The catalyst is a solid superbase catalyst K2O / SnO2-ZrO2.
[0009] In the present invention, the solid superbase catalyst K2O / SnO2-ZrO2 has a K2O mass fraction of 20% to 45%, a SnO2 mass fraction of 35% to 60%, and a ZrO2 mass fraction of 5% to 20%.
[0010] In the present invention, the preparation method of the solid super base catalyst comprises the following steps: taking soluble salts of tin and zirconium and adding them into water to dissolve them, then adding KOH solution thereto, adjusting the pH to 9-11, continuously stirring and refluxing for 2-8 hours under boiling state, filtering the solution to obtain a solid, drying and calcining to obtain a solid super base catalyst K2O / SnO2-ZrO2.
[0011] In the present invention, the soluble salts of tin and zirconium are tin nitrate and zirconium nitrate.
[0012] In the present invention, the drying temperature ranges from 100 to 160° C., the drying time is 4 to 10 hours, the calcination temperature ranges from 400 to 600° C., and the calcination time is 1 to 5 hours.
[0013] As a preferred solution, the preparation method is as follows: weigh 3-6g Sn(NO3)4 and 0.4-3.2g Zr(NO3)4, add them into 100ml deionized water, and stir for 10-20min until fully dissolved. Add 2-8% KOH solution, adjust the pH to 9-11, continue stirring and refluxing for 8h under boiling state, filter the solution to obtain solid, and dry it in an oven at 120℃ for 8h. Take out the solid, raise the temperature from room temperature to 500℃ in a muffle furnace, and calcine for 3h to obtain the solid super base catalyst K2O / SnO2-ZrO2.
[0014] In the present invention, the alcohol is generally methanol, and can also be ethanol, propanol, ethylene glycol, propylene glycol, etc., and the corresponding products obtained are dimethyl carbonate, dipropyl carbonate, diethylene glycol carbonate and dipropylene glycol carbonate. The polycarbonate can be bisphenol A type polycarbonate, fatty polycarbonate, such as polyethylene carbonate, polytrimethylene carbonate, etc., preferably bisphenol A type polycarbonate.
[0015] In the present invention, the solvent is one or more of dichloromethane, dichloroethane, carbon tetrachloride, dioxane, tetrahydrofuran, and acetone. Polycarbonate has excellent solubility in the above solvents, and the alcoholysis reaction time, temperature and other conditions are improved.
[0016] In the present invention, a mixed solution is prepared according to the mass ratio of waste polycarbonate: alcohol: solvent: catalyst of 1: (1-10): (5-20): (0.01-0.5).
[0017] Furthermore, the mixed solution is heated at 20° C. to 150° C. for 2 h to 8 h, and the waste polycarbonate can be completely degraded into bisphenol A and dimethyl carbonate.
[0018] Furthermore, the product was centrifuged to obtain a solid catalyst, which was reused 10 times and still had excellent catalytic performance.
[0019] Furthermore, the liquid phase products are distilled according to their boiling point differences to obtain bisphenol A and carbonate products.
[0020] As a preferred scheme, a method for catalyzing the degradation of waste polycarbonate using a solid superbase is provided, wherein the catalyst is a solid superbase catalyst K2O / SnO2-ZrO2, and a mixed solution is prepared under the condition that the mass ratio of waste polycarbonate: alcohol: solvent: catalyst is 1: (1-10): (5-20): (0.01-0.5), and the mixed solution is heated at 20°C to 150°C for 2h to 8h. The waste polycarbonate can be completely degraded into bisphenol A (BPA) and carbonate, and the product can be obtained after operations such as centrifugal distillation, and the catalyst can be reused.
[0021] In the present invention, the waste polycarbonate can be a waste polycarbonate product in the form of flakes, particles, strips, etc.
[0022] Taking methanol as an example, the polycarbonate degradation reaction equation is as follows:
[0023]
[0024] The catalytic mechanism of the solid superbase catalyst in the alcoholysis of polycarbonate is that the oxygen atom on the alkoxy group on the ester bond of polycarbonate contains a lone pair of electrons, which can form an unstable intermediate complex with the empty orbitals on the Sn and Zr ions in the catalyst, increasing the positive charge of the carbonyl carbon atom, making it easier for the lone pair of electrons on the oxygen atom in the alcohol to react with the carbon atom to form a nucleophilic bond. At the same time, the CO bond breaks, and the oxygen atom combines with the hydrogen on the methanol, thereby causing an alcoholysis reaction.
[0025] The solid superbase catalyst of the present invention is a heterogeneous catalyst, and its properties do not change after the degradation reaction. It is easy to separate the solid from the liquid product by centrifugation or filtration, which solves the problem that the traditional homogeneous alkaline catalyst cannot be reused and the residue in the product may affect the further application of the product. The catalyst preparation method is simple, the cost is low, and after being reused 10 times, its catalytic performance is still excellent.
[0026] The positive effects of the present invention are:
[0027] (1) A method for chemically recovering waste polycarbonate was developed. Through a mild catalytic alcoholysis process, waste polycarbonate was degraded into bisphenol compounds and carbonate compounds, thus realizing the resource utilization of waste plastics.
[0028] (2) The solid superbase catalyst of the present invention has a simple preparation method and low cost, and its catalytic performance is still excellent after being reused for more than 10 times, which solves the problem that the traditional homogeneous alkaline catalyst cannot be reused and the residue in the product may affect the further application of the product. DETAILED DESCRIPTION
[0029] The present invention is further described in detail below through specific examples, but they should not be construed as limiting the present invention.
[0030] Waste polycarbonate is taken from a waste pure water barrel (18.9L specification), which is cut and crushed to a certain size. Other chemicals used in the catalytic alcoholysis of polycarbonate are all chemically pure drugs.
[0031] Polycarbonate depolymerization rate = (1-polycarbonate residual amount / polycarbonate added amount) ╳ 100%
[0032] Yield of bisphenol A (carbonate) = amount of bisphenol A (carbonate) in the product / amount of bisphenol A (carbonate) generated by complete degradation of the added polycarbonate × 100%
[0033] In the following examples, % is by weight unless otherwise specified.
[0034] The metal content in the solid superbase catalyst is quantitatively analyzed by ICP, the dimethyl carbonate content is analyzed by gas chromatography, and the bisphenol A content is analyzed by liquid chromatography. The following are the equipment models and detailed parameters.
[0035] Table 1. ICP analysis conditions for metal content
[0036]
[0037] Table 2. Gas chromatography analysis method parameters
[0038]
[0039]
[0040] Table 3 Parameters of liquid chromatography BPA analysis method
[0041]
[0042]
[0043] Example 1
[0044] The preparation method of solid superbase K2O / SnO2-ZrO2 is as follows: weigh 4.3g Sn(NO3)4 and 2.8g Zr(NO3)4, add them to 100ml deionized water successively, and stir for 15min until fully dissolved. Add 135.5g of 2% KOH solution, adjust the pH to 11, continue stirring and refluxing for 8h under boiling state, filter the solution to obtain solid, and dry it in an oven at 120℃ for 8h. Take out the solid, raise the temperature from room temperature to 500℃ in a muffle furnace, and calcine for 3h to obtain the solid superbase catalyst K2O / SnO2-ZrO2, in which the mass fraction of K2O is 45%, the mass fraction of SnO2 is 35%, and the mass fraction of ZrO2 is 20%. A mixed solution was prepared under the condition that the mass ratio of waste polycarbonate: methanol: dichloromethane: catalyst was 1:3:5:0.05, and heated at 20°C for 8 hours. After the experiment, the product was filtered to obtain the catalyst and liquid phase product, and the content of bisphenol A and dimethyl carbonate was analyzed (see Table 2 and Table 3 for the analysis method). It was calculated that the depolymerization rate of polycarbonate was 94.5%, the yield of BPA was 92.8%, and the yield of DMC was 91.6%. After the catalyst was filtered and recovered, the above steps were repeated ten times to verify the catalyst performance. The depolymerization rate of polycarbonate was above 94%, confirming that the catalyst performance was not significantly attenuated.
[0045] Example 2
[0046] The preparation method of solid superbase K2O / SnO2-ZrO2 is as follows: weigh 5.3g Sn(NO3)4 and 0.5g Zr(NO3)4, add them to 100ml deionized water successively, and stir for 15min until fully dissolved. Add 50.5g 3% KOH solution, adjust the pH to 10, continue stirring and refluxing for 8h under boiling state, filter the solution to obtain solid, and dry it in an oven at 120℃ for 8h. Take out the solid, raise the temperature from room temperature to 500℃ in a muffle furnace, and calcine for 3h to obtain solid superbase catalyst K2O / SnO2-ZrO2. The mass fraction of K2O is 35%, the mass fraction of SnO2 is 60%, and the mass fraction of ZrO2 is 5%. A mixed solution was prepared under the condition that the mass ratio of waste polycarbonate: methanol: tetrahydrofuran: catalyst was 1: 5: 10: 0.1, and heated at 50 ° C for 6 hours. After the experiment, the product was filtered to obtain the catalyst and liquid phase product, and the content of bisphenol A and dimethyl carbonate was analyzed (see Table 2 and Table 3 for the analysis method). It was calculated that the depolymerization rate of polycarbonate was 95.6%, the yield of BPA was 94.8%, and the yield of DMC was 93.7%. After the catalyst was filtered and recovered, the above steps were repeated ten times to verify the catalyst performance. The depolymerization rate of polycarbonate was above 95%, which confirmed that the catalyst performance was not significantly attenuated.
[0047] Example 3
[0048] The preparation method of solid superbase K2O / SnO2-ZrO2 is as follows: weigh 4.9g Sn(NO3)4 and 1.8g Zr(NO3)4, add them to 100ml deionized water successively, and stir for 15min until fully dissolved. Add 16.0g of 5% KOH solution, adjust the pH to 9, continue stirring and refluxing for 8h under boiling state, filter the solution to obtain solid, and dry it in an oven at 120℃ for 8h. Take out the solid, raise the temperature from room temperature to 500℃ in a muffle furnace, and calcine for 3h to obtain the solid superbase catalyst K2O / SnO2-ZrO2. The mass fraction of K2O is 20%, the mass fraction of SnO2 is 60%, and the mass fraction of ZrO2 is 20%. A mixed solution was prepared under the condition that the mass ratio of waste polycarbonate: methanol: dioxane: catalyst was 1:9:15:0.3, and heated at 100°C for 4 hours. After the experiment, the product was filtered to obtain the catalyst and liquid phase product, and the content of bisphenol A and dimethyl carbonate therein was analyzed (see Table 2 and Table 3 for the analysis method). It was calculated that the depolymerization rate of polycarbonate was 98.7%, the yield of BPA was 96.2%, and the yield of DMC was 94.1%. After the catalyst was filtered and recovered, the above steps were repeated ten times to verify the catalyst performance. The depolymerization rate of polycarbonate was above 98%, which confirmed that the catalyst performance was not significantly attenuated.
[0049] Example 4
[0050] The preparation method of solid superbase K2O / SnO2-ZrO2 is as follows: weigh 4.3g Sn(NO3)4 and 2.8g Zr(NO3)4, add them to 100ml deionized water successively, and stir for 15min until fully dissolved. Add 54.2g of 5% KOH solution, adjust the pH to 11, continue stirring and refluxing for 6h under boiling state, filter the solution to obtain solid, and dry it in an oven at 120℃ for 8h. Take out the solid, raise the temperature from room temperature to 500℃ in a muffle furnace, and calcine for 3h to obtain solid superbase catalyst K2O / SnO2-ZrO2, in which the mass fraction of K2O is 45%, the mass fraction of SnO2 is 35%, and the mass fraction of ZrO2 is 20%. A mixed solution was prepared under the condition that the mass ratio of waste polycarbonate: methanol: ethylene dichloride: catalyst was 1:10:20:0.5, and heated at 150°C for 2h. After the experiment, the product was filtered to obtain the catalyst and liquid phase product, and the content of bisphenol A and dimethyl carbonate was analyzed (see Table 2 and Table 3 for the analysis method). It was calculated that the depolymerization rate of polycarbonate was 99.5%, the yield of BPA was 98.3%, and the yield of DMC was 94.5%. After the catalyst was filtered and recovered, the above steps were repeated ten times to verify the catalyst performance. The depolymerization rate of polycarbonate was above 99%, which confirmed that the catalyst performance was not significantly attenuated.
[0051] Example 5
[0052] The preparation method of solid superbase K2O / SnO2-ZrO2 is as follows: weigh 4.9g Sn(NO3)4 and 1.8g Zr(NO3)4, add them to 100ml deionized water successively, and stir for 15min until fully dissolved. Add 10.0g 8% KOH solution, adjust the pH to 9, continue stirring and refluxing for 8h under boiling state, filter the solution to obtain solid, and dry it in an oven at 120℃ for 8h. Take out the solid, raise the temperature from room temperature to 500℃ in a muffle furnace, and calcine for 3h to obtain the solid superbase catalyst K2O / SnO2-ZrO2. The mass fraction of K2O is 20%, the mass fraction of SnO2 is 60%, and the mass fraction of ZrO2 is 20%. A mixed solution was prepared under the condition that the mass ratio of waste polycarbonate: ethylene glycol: dichloromethane: catalyst was 1:5:15:0.1, and heated at 120°C for 3 hours. After the experiment, the product was filtered to obtain the catalyst and liquid phase product, and the content of bisphenol A and diethylene glycol carbonate was analyzed (see Table 2 and Table 3 for the analysis method). It was calculated that the depolymerization rate of polycarbonate was 98.4%, the yield of BPA was 96.8%, and the yield of DMC was 93.8%. After the catalyst was filtered and recovered, the above steps were repeated ten times to verify the catalyst performance. The depolymerization rate of polycarbonate was above 98%, which confirmed that the catalyst performance was not significantly attenuated.
Claims
1. A method for catalytic degradation of waste polycarbonate using a solid superbase, characterized in that: A mixed solution of waste polycarbonate, alcohol, solvent and catalyst is prepared, wherein the mass ratio of waste polycarbonate: alcohol: solvent: catalyst is 1: (1-10): (5-20): (0.01-0.5), and the mixture is heated at 20°C-150°C for 2h-8h to degrade the waste polycarbonate into bisphenol compounds and carbonate compounds. After post-treatment, a product is obtained. The catalyst is a solid super base catalyst K2O / SnO2-ZrO2, wherein the mass fraction of K2O is 20%-45%, the mass fraction of SnO2 is 35%-60%, and the mass fraction of ZrO2 is 5%-20%.
2. The method according to claim 1, characterized in that: The preparation method of the solid super base catalyst comprises the following steps: taking soluble salts of tin and zirconium and adding them into water to dissolve them, then adding KOH solution thereto, adjusting the pH to 9-11, continuously stirring and refluxing under boiling state for 2-8 hours, filtering the solution to obtain a solid, drying and calcining to obtain a solid super base catalyst K2O / SnO2-ZrO2.
3. The method according to claim 2, characterized in that: The drying temperature ranges from 100 to 160°C, the drying time is 4 to 10 hours, the calcination temperature ranges from 400 to 600°C, and the calcination time is 1 to 5 hours.
4. The method according to claim 1, characterized in that: The alcohol is one or more of methanol, ethanol, propanol, ethylene glycol and propylene glycol, and the corresponding products are dimethyl carbonate, dipropyl carbonate, diethylene glycol carbonate and dipropylene glycol carbonate.
5. The method according to claim 1, characterized in that: The solvent is one or more of dichloromethane, dichloroethane, carbon tetrachloride, dioxane, tetrahydrofuran and acetone.
6. The method according to claim 1, characterized in that: The post-processing operation is to distill the alcoholysis product according to the difference in boiling points to obtain a refined product.