Indole polyketone and preparation method thereof

By preparing indole-based polyketides, the problems of difficult removal of impurities and insufficient performance in the preparation process of polyether ether ketones were solved, and the high temperature resistance and mechanical properties were significantly improved, meeting the application requirements of high-performance engineering plastics.

CN116239768BActive Publication Date: 2024-11-08SHANDONG TIANWEI MEMBRANE TECH
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202310045705.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-01-30
Publication Date
2024-11-08
Estimated Expiration
2043-01-30

AI Technical Summary

Technical Problem

The existing preparation process of polyetheretherketone is cumbersome, metal impurities are difficult to completely remove, and mechanical properties are insufficient, which cannot meet the application requirements of high-performance engineering plastics.

Method used

By using indole polyketides as alternative materials, and through polymerization catalyzed by phosphorus pentoxide and methanesulfonic acid, the introduction of metal salt catalysts is avoided, the reaction temperature is reduced, and the purification steps are simplified, thus preparing indole polyketides with excellent high-temperature resistance and mechanical properties.

Benefits of technology

Indole polyketides have an initial thermal decomposition temperature of over 430℃ and a tensile strength of over 150MPa, significantly improving their mechanical properties and meeting the application requirements of high-performance engineering plastics.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116239768B_ABST
    Figure CN116239768B_ABST
Patent Text Reader

Abstract

The present invention belongs to the field of high-performance polymer applications, and specifically relates to an indole polyketone and a preparation method thereof. The preparation method of the indole polyketone proposed by the present invention not only has a simple preparation process, can carry out polymerization reaction at a temperature of 20-100°C, but also avoids the introduction of a metal salt catalyst, so that the product does not contain metal ion impurities, which is convenient for subsequent purification treatment, and the prepared indole polyketone has good mechanical properties and high temperature resistance, the tensile strength can reach more than 150MPa, and the initial thermal decomposition temperature is above 430°C, which can meet the application requirements of high-performance engineering plastics.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of high-performance polymer applications, and specifically relates to an indole polyketone and a preparation method thereof. Background Art

[0002] As a type of polyaryletherketone, polyetheretherketone has good heat resistance, chemical corrosion resistance and mechanical properties, as well as radiation resistance, fatigue resistance, wear resistance and other advantages. As a high-performance engineering plastic, it is widely used in aerospace, electronic products, military, communications and many other fields. However, due to the easy crystallization of polyetheretherketone itself, the synthesis and preparation process is relatively difficult.

[0003] At present, difluorobenzophenone and hydroquinone are usually used as raw materials, and polyetheretherketone is prepared by polymerization reaction in a high boiling point solvent under the catalysis of potassium carbonate or calcium carbonate. For example, the Chinese invention patent with application publication number CN105482050A discloses a method for preparing polyetheretherketone resin, using 4,4′-difluorobenzophenone and hydroquinone as raw materials, potassium carbonate and calcium carbonate as catalysts, first reacting at 220°C for 2 hours, and then heating to 310°C for polymerization reaction for 2.5 hours to obtain polyetheretherketone. However, in this method, the polymerization reaction of dicalcium hydroquinone and 4,4′-difluorobenzophenone needs to be carried out at 310°C. In addition, the impurity removal step of the obtained product polyetheretherketone is very cumbersome, and the trace metal salts included are difficult to be thoroughly cleaned. In addition, the tensile strength of the product polyetheretherketone is 89-95Mpa, which is gradually unable to meet the increasing application needs in the field of engineering plastics.

[0004] Therefore, there is an urgent need for an engineering plastic with a simple preparation method and excellent performance to replace the application of polyetheretherketone. Summary of the invention

[0005] The object of the present invention is to provide an indole polyketone to solve the problem of poor mechanical properties of polyetheretherketone in the prior art.

[0006] The second object of the present invention is to provide a method for preparing indole polyketones, so as to solve the problems of harsh preparation conditions and difficulty in removing metal impurities in the preparation process of polyetheretherketone in the prior art.

[0007] In order to achieve the above object, the present invention provides an indole polyketone, which includes a structural unit as shown in Formula 1:

[0008]

[0009]

[0010] R1 is selected from -H or C1-C3 alkyl.

[0011] The indole polyketone proposed in the present invention not only has a simple structure and excellent high temperature resistance, but also has better mechanical properties than polyetheretherketone because the main chain of the indole polyketone is completely composed of a rigid indole ring connected to a carbonyl group. Experimental verification shows that the tensile strength can reach above 150MPa and the initial thermal decomposition temperature can reach above 430°C, which can meet the current application requirements of high-performance engineering plastics.

[0012] The above-mentioned indole polyketone may also contain other structural units that introduce indole rings and / or carbonyl groups into the main chain. Furthermore, the above-mentioned indole polyketone also includes a structural unit as shown in Formula 2:

[0013]

[0014] R2 in Formula 2 is selected from -H or a C1-C3 alkyl group; R2 in Formula 2 is different from R1 in Formula 1.

[0015] The molecular weight of the indole polyketone in the present invention is characterized by the logarithmic viscosity of the concentration. Preferably, the logarithmic viscosity of the indole polyketone is 0.5 dL / g to 5 dL / g. The logarithmic viscosity is measured by the following steps: using methanesulfonic acid as a solvent, the indole polyketone is prepared into a solution with a concentration of 0.5 g / dL, and the logarithmic viscosity is measured using an Ubbelohde viscometer at a temperature of 25°C.

[0016] Preferably, the inherent viscosity of the indole polyketone is 3.0 to 5.0 dL / g.

[0017] The preparation method of an indole polyketone of the present invention comprises the following steps: subjecting a comonomer to a polymerization reaction under the catalytic action of phosphorus pentoxide and methanesulfonic acid; the comonomer is a compound shown in Formula 3 and / or a compound shown in Formula 4:

[0018]

[0019]

[0020] R3 in Formula 3 is -H; R4 in Formula 4 is selected from a C1-C3 alkyl group.

[0021] The preparation method of the indole polyketone proposed by the present invention uses the comonomer shown in Formula 4 as a raw material, and generates the indole polyketone through a Fusorial acylation reaction under the catalysis of phosphorus pentoxide and methanesulfonic acid, which not only greatly reduces the temperature required for the reaction, but also avoids the introduction of metal salt catalysts, so that the product does not contain metal ion impurities, which is convenient for subsequent purification. The obtained indole polyketone has a thermal decomposition temperature of more than 430°C and a tensile strength of more than 150MPa, and has thermal and mechanical properties comparable to those of polyetheretherketone in the prior art, and can meet the application requirements of high-performance engineering plastics.

[0022] Preferably, the preparation method of indole polyketone proposed in the present invention can achieve polymerization at a relatively low temperature, the polymerization reaction temperature is 20 to 100° C., and the reaction time is 3 to 24 hours.

[0023] Preferably, the polymerization reaction is carried out under anhydrous conditions in order to avoid failure caused by reaction of phosphorus pentoxide with water during the reaction process.

[0024] Preferably, a mixture of phosphorus pentoxide and methanesulfonic acid can be obtained in advance, and then the comonomer and the mixture of phosphorus pentoxide and methanesulfonic acid are mixed to carry out polymerization reaction. Furthermore, the mixture of phosphorus pentoxide and methanesulfonic acid can be a commercial product or homemade, and the preparation method is as follows: phosphorus pentoxide and methanesulfonic acid are mixed in proportion.

[0025] Preferably, the mass ratio of phosphorus pentoxide to methanesulfonic acid is 7 to 10:100, and the ratio of the mass of the comonomer to the total mass of phosphorus pentoxide and methanesulfonic acid is 1 to 6:20.

[0026] Preferably, the preparation method of the indole polyketone of the present invention further comprises the following steps: after the polymerization reaction is completed, the polymerization product is washed and dried to achieve purification of the indole polyketone. Further, the polymerization product is washed and dried by the following steps: the polymerization product is slowly added into water, allowed to stand, the obtained precipitate is extracted with water through an extractor for 24-48 hours, and finally vacuum dried at 100° C. for 24 hours to obtain the indole polyketone. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 This is the hydrogen nuclear magnetic resonance spectrum of the product obtained in Experimental Example 1 of the present invention. DETAILED DESCRIPTION

[0028] The technical solution of the present invention is further described in detail below in conjunction with specific implementation methods.

[0029] 1. The embodiments of the indole polyketone of the present invention are as follows:

[0030] The inherent viscosity (V inh ) was measured by the Ubbelohde viscometer method, using methanesulfonic acid as the solvent to prepare a solution with a concentration of 0.5 g / L, and the test temperature was 25°C.

[0031] Example 1

[0032] The structural unit of the indole polyketone of this embodiment is shown in Formula 5, and the measured inherent viscosity of the indole polyketone is 3.0 dL / g. The indole polyketone of this embodiment is prepared by the preparation method of the indole polyketone in Example 4.

[0033]

[0034] Example 2

[0035] The structural unit of the indole polyketone of this embodiment is shown in Formula 6. The measured inherent viscosity of the indole polyketone is 4.4 dL / g. The indole polyketone of this embodiment is prepared by the preparation method of the indole polyketone in Example 5.

[0036]

[0037] Example 3

[0038] The structural units of the indole polyketone of this embodiment are shown in Formula 5 and Formula 6. The measured inherent viscosity of the indole polyketone is 5.0 dL / g. The indole polyketone of this embodiment is prepared by the preparation method of the indole polyketone in Example 6.

[0039] 2. The embodiment of the preparation method of the indole polyketone of the present invention is as follows:

[0040] Example 4

[0041] The preparation method of the indole polyketone of this embodiment is the preparation method of the indole polyketone in Example 1, which specifically comprises the following steps: nitrogen is introduced into a glass reactor to replace the air, and then 1 kg of 6-indolecarboxylic acid and 20 kg of a mixture of phosphorus pentoxide and methanesulfonic acid (the mass ratio of phosphorus pentoxide to methanesulfonic acid is 7:100) are added to the glass reactor, and mechanically stirred at 20°C for 24 hours to allow it to fully undergo a polymerization reaction.

[0042] The obtained viscous reaction solution was slowly added into water, and allowed to stand for precipitation. The obtained precipitate was extracted with water through an extractor for 48 hours, and finally vacuum dried at 100°C for 24 hours to obtain indole polyketone. The polymerization reaction formula is shown below:

[0043]

[0044] Example 5

[0045] The preparation method of the indole polyketone of this embodiment is the preparation method of the indole polyketone in Example 2, which specifically comprises the following steps: nitrogen is introduced into a glass reactor to replace the air, and then 1 kg of 1-methyl-6-indolecarboxylic acid and 10 kg of a mixture of phosphorus pentoxide and methanesulfonic acid (the mass ratio of phosphorus pentoxide to methanesulfonic acid is 8.5:100) are added to the glass reactor, and mechanically stirred at 80° C. for 8 hours to allow it to fully undergo a polymerization reaction.

[0046] The obtained viscous reaction solution was slowly added into water, and allowed to stand for precipitation. The obtained precipitate was extracted with water through an extractor for 24 hours, and finally vacuum dried at 100°C for 24 hours to obtain indole polyketone. The polymerization reaction formula is shown below:

[0047]

[0048] Example 6

[0049] The preparation method of the indole polyketone of this embodiment is the preparation method of the indole polyketone in Example 3, which specifically comprises the following steps: nitrogen is introduced into a glass reactor to replace the air, and then 1.61 kg of 1-methyl-6-indolecarboxylic acid, 1.75 kg of 6-indolecarboxylic acid, and 11.2 kg of a mixture of phosphorus pentoxide and methanesulfonic acid (the mass ratio of phosphorus pentoxide to methanesulfonic acid is 10:100) are added to the glass reactor, and mechanically stirred at 100° C. for 3 hours to allow it to fully undergo a polymerization reaction.

[0050] The obtained viscous reaction liquid was slowly added into water and allowed to stand for precipitation. The obtained precipitate was extracted with water through an extractor for 24 hours and finally vacuum dried at 100° C. for 24 hours to obtain indole polyketone.

[0051]

[0052] 3. Experimental Examples

[0053] Experimental Example 1

[0054] This experimental example is used to verify the feasibility of preparing indole sulfonated polymers by using a comonomer and a mixture of phosphorus pentoxide and methanesulfonic acid through a acylation reaction in the present invention. Specifically, the following steps are included: 0.832g (4.75mmol) of methyl 6-indolecarboxylate, 1.445g (9.50mmol) of 4-methoxybenzoic acid and 25g of a phosphorus pentoxide / methanesulfonic acid mixture (phosphorus pentoxide to methanesulfonic acid weight ratio is 7:100) are added to a dry three-necked flask with nitrogen, stirred at 60°C for 1 hour, and then the reaction product is added to 100mL of ice water and allowed to stand. The resulting precipitate is washed with water, a NaHCO3 solution with a concentration of 0.1mol / L, and water in turn, and finally vacuum dried at 80°C for 24 hours to obtain 1.43g of yellow powder with a yield of 97%. The polymerization reaction formula is shown below:

[0055]

[0056] The product obtained in this example was tested by hydrogen nuclear magnetic resonance spectrum using deuterated dimethyl sulfoxide as solvent and tetramethylsilane as internal standard. The results are as follows: Figure 1 In this Experimental Example 1, a 3-acylated indole derivative was obtained with a yield of 97%, and the nitrogen and other positions on the indole ring did not undergo acylation reaction with 4-methoxybenzoic acid (even in the presence of excess 4-methoxybenzoic acid), indicating that the acylation reaction occurred quantitatively and selectively at the 3-position of the indole ring.

[0057] Experimental Example 2

[0058] This experimental example is used to test the performance of the indole polyketone in Examples 1-3, specifically including:

[0059] 1. The initial decomposition temperature of indole polyketone in air was tested by thermogravimetric analysis, with the temperature rising from room temperature to 800°C at a rate of 10°C / min.

[0060] 2. The tensile properties of indole polyketone were tested according to GB / T1040.1-2006. The results are shown in Table 1, wherein the samples were prepared by compression molding.

[0061] Table 1

[0062] Initial decomposition temperature Tensile Strength Elongation at break Example 1 460℃ 187MPa 9.6% Example 2 446℃ 160MPa 8.8% Example 3 430℃ 150MPa 13.6%

[0063] The experimental results show that the initial thermal decomposition temperature of the indole polyketone proposed in the present invention reaches above 430°C, the tensile strength reaches above 150MPa, and the elongation at break is below 13.6%. Its mechanical properties are greatly improved compared with those of polyetheretherketone, and it has a large application space in the field of high-performance engineering plastics.

Claims

1. An indole polyketone, characterized in that: The indole polyketone comprises a structural unit as shown in Formula 1: R1 is selected from -H or C1-C3 alkyl.

2. The indole polyketone according to claim 1, characterized in that: The indole polyketone further comprises a structural unit as shown in Formula 2: R2 in Formula 2 is selected from -H or a C1-C3 alkyl group; R2 in Formula 2 is different from R1 in Formula 1.

3. The indole polyketone according to any one of claims 1 to 2, characterized in that: The inherent viscosity of the indole polyketone is 0.5-5.0 dL / g; the inherent viscosity is measured by the following steps: using methanesulfonic acid as a solvent, preparing the indole polyketone into a solution with a concentration of 0.5 g / dL, and measuring the inherent viscosity using an Ubbelohde viscometer at a temperature of 25°C.

4. The indole polyketone according to claim 3, characterized in that: The inherent logarithmic viscosity of the indole polyketone is 3.0-5.0 dL / g.

5. A method for preparing an indole polyketone, characterized in that: The following steps are involved: The comonomer is polymerized under the catalytic action of phosphorus pentoxide and methanesulfonic acid; the comonomer is a compound shown in Formula 3 and / or a compound shown in Formula 4: R3 in Formula 3 is -H; R4 in Formula 4 is selected from a C1-C3 alkyl group.

6. The method for preparing indole polyketone according to claim 5, characterized in that: The polymerization reaction temperature is 20 to 100° C., and the reaction time is 3 to 24 hours.

7. The method for preparing an indole polyketone according to any one of claims 5 to 6, characterized in that: The mass ratio of phosphorus pentoxide to methanesulfonic acid is 7-10:100; the mass ratio of the copolymer monomer to the total mass of phosphorus pentoxide and methanesulfonic acid is 1-6:

20.

8. The method for preparing an indole polyketone according to any one of claims 5 to 6, characterized in that: The following steps are also included: After the polymerization reaction is completed, the polymerization product is washed and dried.

Citation Information

Patent Citations

  • Method for preparing polyether ether ketone

    CN105482050A

  • Aromatic sulfonated poly ketone and preparation method thereof

    CN103709379A

  • Thermotropic main chain type crystal liquid polyketone and preparation method thereof

    CN104530341A

  • Polyketone indole alkaloid as well as preparation method and application thereof

    CN109096263A

  • Synthesis method of polyketone

    CN110684189A