A high-strength bacterial cellulose-based hydrogel with antifreeze and moisture retention, and preparation method and application thereof
Through the polymer hydrogel technology of bacterial cellulose and N-acryloyl aspartic acid and other components, combined with the glycerol/water solution system, a high-density hydrogen bond network is formed, which solves the problem that traditional hydrogels are easy to freeze and freeze at low temperatures. It solves the problem of water loss, achieves high strength and long life anti-freeze and moisturizing effects, and provides an effective repair material for harsh medical environments.
Patent Information
- Application Number
- CN202310246771.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-14
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2043-03-14
AI Technical Summary
Traditional hydrogels are prone to freezing at low temperatures and their structures are prone to collapse, resulting in short service life and inability to effectively resist freezing and moisturizing in harsh medical environments.
It uses components such as bacterial cellulose, N-[tris(hydroxymethyl)methyl]acrylamide and N-acryloyl aspartic acid, and is initiated by ultraviolet light to form a polymer hydrogel, which is combined with a glycerol/water solution system to form High-density hydrogen bonding network for enhanced tensile strength and moisturizing properties.
A high-strength bacterial cellulose-based hydrogel that is anti-freeze and moisturizing is prepared, with a tensile strength of 6.75MPa and low water loss rate. It can maintain structural integrity in low-temperature environments, extend service life, and has good biocompatibility. sex.
Smart Images

Figure CN116239800B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of gel production, and particularly relates to a high-strength bacterial cellulose-based hydrogel with antifreeze and moisture retention, and a preparation method and application thereof. Background Art
[0002] As the first natural barrier of the human body against external stimuli, the skin will face various external hazards, such as wounds, burns, chronic ulcers, etc. Once the skin is damaged, it will cause problems such as delayed healing and infection, seriously damaging the comprehensive barrier function of the skin and individual health. In recent years, hydrogels, as a network polymer with high water content, have been widely used in the field of wound repair due to their good biocompatibility and easy functionalization. However, traditional hydrogels using pure water as a dispersion medium generally have two disadvantages: the first disadvantage is that they are easy to freeze at low temperatures, which greatly limits the activity of hydrogels at low temperatures. The other is the structural collapse caused by water evaporation, which greatly shortens the life of the hydrogel in an open environment. Therefore, the development of a new type of hydrogel that can simultaneously achieve antifreeze and moisturizing functions is expected to be used in some harsh medical environments. Summary of the invention
[0003] The purpose of the present invention is to solve the above technical problems and to provide a high-strength bacterial cellulose-based hydrogel with excellent antifreeze and moisturizing properties, tensile strength and good biocompatibility, as well as a preparation method and application thereof.
[0004] The purpose of the present invention can be achieved through the following technical scheme: a high-strength bacterial cellulose-based hydrogel with antifreeze and moisture retention, comprising the following components in parts by weight: 5-10 parts of bacterial cellulose, 10-20 parts of N-[tris(hydroxymethyl)methyl]acrylamide (THMA), and 20-30 parts of N-acryloyl aspartic acid (AASP).
[0005] Furthermore, the N-acryloyl aspartic acid is prepared by the following method:
[0006] Aspartic acid and sodium hydroxide are dissolved in ice-cold deionized water in a mass ratio of 8-10:7-9, and the reaction condition is an ice bath; acryloyl chloride and polar solvent are fully mixed in a volume ratio of 7-9:15-19, and added dropwise to the above solution, during the reaction, the pH is maintained at a weak alkaline, and further reacted at room temperature for 3-5h; the pH of the mixture is adjusted to alkaline conditions with NaOH with a concentration of 2-5M, washed with ethyl acetate to remove the organic phase, and the pH of the aqueous phase is adjusted to acidic conditions with HCl with a concentration of 3-6M, and then the aqueous phase is extracted again with ethyl acetate, the organic layer is dried with magnesium sulfate, filtered, concentrated, and precipitated in n-hexane, and the precipitation is repeated for further purification, and the collected product is dried in a vacuum. The N-acryloyl aspartic acid prepared by this method retains the good biocompatibility of aspartic acid, and at the same time has a carbon-carbon double bond, cross-linked with THMA under the initiation of ultraviolet light to form a high molecular weight hydrogel polymer, and is firmly bonded to bacterial cellulose through the action of hydrogen bonds, and has good tensile strength.
[0007] Furthermore, the polar solvent includes dimethyl sulfoxide, tetrahydrofuran or dimethylformamide.
[0008] The present invention also provides a method for preparing a high-strength bacterial cellulose-based hydrogel with antifreeze and moisture retention, comprising the following steps:
[0009] The bacterial cellulose is first prepared into a film by weight, and then N-[tri(hydroxymethyl)methyl]acrylamide and N-acryloyl aspartic acid are added to a mixed solution system of glycerol and water, and a cross-linking agent and an initiator are added. After fully dissolved, the bacterial cellulose film is immersed in the above solution, and polymerized under ultraviolet light and anaerobic conditions to obtain a high-strength bacterial cellulose-based hydrogel with antifreeze and moisture retention.
[0010] Based on the total mass of bacterial cellulose, N-tris(hydroxymethyl)methyl]acrylamide and N-acryloyl aspartic acid as 100, the mass percentage of the crosslinking agent is 0.01-0.02%, and the mass percentage of the initiator is 0.02-0.03%. The polymerization conditions are ultraviolet light source and oxygen-free.
[0011] Furthermore, the cross-linking agent is one or more of polyethylene glycol diacrylate, N,N-methylenebisacrylamide, cyclotriene bond, and triallyl isocyanurate.
[0012] Furthermore, the initiator is one or more of 2-hydroxy-2-methylpropiophenone, ammonium persulfate, and α-ketoglutaric acid.
[0013] Furthermore, the volume ratio of glycerol to water in the mixed solution of glycerol and water is 1:1.
[0014] The present invention also provides an application of a high-strength bacterial cellulose-based hydrogel that is antifreeze and moisturizing, which is used in the fields of biological tissue engineering and clinical treatment, especially in the repair of tissue defects.
[0015] Compared with the prior art, the present invention has the following advantages:
[0016] (1) The present invention uses bacterial cellulose film as a base template to prepare a hydrogel with a tensile strength of up to 6.75 MPa. The bacterial cellulose fibers are composed of microfibers with a diameter of 3 to 4 nanometers combined into fiber bundles with a thickness of 40 to 60 nanometers, which are interwoven to form a developed ultra-fine network structure. When the bacterial cellulose solution is filtered to prepare a film, the bacterial cellulose is interwoven and stacked more tightly, and the strength is increased. It is immersed in a hydrogel precursor solution and polymerized under the initiation of ultraviolet light to prepare a composite product. The tensile strength of the final composite product is increased;
[0017] (2) The antifreeze and moisturizing high-strength bacterial cellulose-based hydrogel prepared by the present invention uses a glycerol / water mixed system as a solvent. Glycerol contains hydroxyl groups and is hydrophilic, so it can be dissolved in water to form a glycerol aqueous solution. When glycerol and water are mixed, a large number of hydrogen bonds are formed between glycerol and water molecules. On the one hand, the orderly arrangement of water molecules is destroyed, so that the freezing point is lowered. On the other hand, a large amount of bound water is formed through the action of hydrogen bonds, which prevents the rapid evaporation of water. The shortcomings of traditional hydrogels such as easy freezing and easy water loss can be effectively solved, so that the bacterial cellulose-based hydrogel prepared by the present invention can be applied to some harsh environments, effectively extending the service life of the hydrogel, and saving a certain amount of economic cost;
[0018] (3) The antifreeze and moisturizing high-strength bacterial cellulose-based hydrogel prepared by the present invention can firmly adhere to the skin tissue through the effect of "hydrogen bond clusters" (the effect of hydrogen bond clusters means that the two carboxyl groups in the AASP monomer and the three hydroxyl groups in the THMA monomer can form hydrogen bonds with the tissue. When the two are polymerized at a certain concentration to form a hydrogel, a large number of carboxyl groups and hydroxyl groups will exist in the hydrogel, and a large number of hydrogen bonds will be formed. These high-density hydrogen bonds will enhance the adhesion between the hydrogel and the tissue in a clustered manner without the need for any chemical reaction);
[0019] (4) The antifreeze and moisture-retaining high-strength bacterial cellulose-based hydrogel prepared by the present invention has good biocompatibility, laying a good foundation for the development of tissue repair materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 The structure and preparation diagram of the material of the present invention;
[0021] Figure 2The hydrogen nuclear magnetic resonance spectrum of N-acryloyl aspartic acid (AASP) prepared by the present invention;
[0022] Figure 3 This is a laser confocal morphology image of the bacterial cellulose-based hydrogel prepared in the present invention;
[0023] Figure 4 This is a graph showing the tensile properties of the bacterial cellulose-based hydrogel prepared in the present invention;
[0024] Figure 5 This is a graph showing the adhesion performance of the bacterial cellulose-based hydrogel prepared in the present invention;
[0025] Figure 6 The antifreeze effect of the bacterial cellulose-based hydrogel prepared by the present invention;
[0026] Figure 7 The moisturizing effect of the bacterial cellulose-based hydrogel prepared by the present invention;
[0027] Figure 8 This is a diagram showing the results of a cytotoxicity test after the bacterial cellulose-based hydrogel prepared in the present invention was co-incubated with L929 cells. DETAILED DESCRIPTION
[0028] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.
[0029] All raw materials used in the present invention are commercially available unless otherwise specified, such as bacterial cellulose, which is a commercially available product and can be selected from Beijing Guanlan Technology Co., Ltd., with a purity greater than 90%. N-[tris(hydroxymethyl)methyl]acrylamide is a commercially available product and can be selected from Shanghai Peter Pharmaceutical Technology Co., Ltd., with a purity greater than 99%.
[0030] The present invention uses nuclear magnetic resonance spectroscopy, a universal tensile testing machine, a confocal microscope, and a cell viability analysis (CCK-8 test) to characterize the bacterial cellulose-based hydrogel prepared by the present invention.
[0031] Example 1
[0032] The specific components and structures of bacterial cellulose-based hydrogels are as follows: Figure 1 As shown, the preparation method comprises the following steps:
[0033] (1) Preparation of N-acryloyl aspartic acid: Aspartic acid (9 g) and sodium hydroxide (8.1 g) were dissolved in 75 mL of deionized water, placed in an ice bath and stirred vigorously. Subsequently, 8 mL of acryloyl chloride and 17.1 mL of tetrahydrofuran were thoroughly mixed and added dropwise to the above reaction system. During the reaction, the pH was maintained at 7-8. The reactants were further stirred at room temperature for 3-4 hours. Subsequently, the pH of the mixture was adjusted to 11 with 3 M NaOH, and then washed with a large amount of ethyl acetate to remove the organic phase. The pH of the aqueous phase was acidified to 2 with 5 M HCl, and then the aqueous phase was extracted again with a large amount of ethyl acetate. The organic layer was dried with magnesium sulfate, filtered, concentrated, and precipitated in n-hexane. The precipitation was repeated for further purification. The test results of nuclear magnetic resonance spectroscopy showed that N-acryloyl aspartic acid ( Figure 2 ), the specific test results are as follows:
[0034] The results of nuclear magnetic resonance spectrum show that N-acryloyl aspartic acid has corresponding proton peak signals at 4.61ppm, 5.64ppm, 6.12ppm, 6.3ppm, 8.13ppm, 2.72ppm and 12.56ppm corresponding to ag in the figure. The test results of nuclear magnetic resonance spectrum show that the present invention successfully synthesizes N-acryloyl aspartic acid.
[0035] (2) Preparation of bacterial cellulose-based hydrogel: First, 200 mL of a bacterial cellulose solution with a mass fraction of 0.4% was filtered and compressed to prepare a bacterial cellulose film, and the film was dried. Then, 0.15 g of N-[tri(hydroxymethyl)methyl]acrylamide and 0.25 g of N-acryloyl aspartic acid were added to 1 mL of a glycerol / water mixed solution system (the ratio of glycerol to water was 1:1), a crosslinker (0.06 mg) and an initiator (0.1 mg) were added, and the dried bacterial cellulose film was immersed in the above mixed solution. After a period of time, it was injected into a mold and irradiated for 20 minutes under oxygen-free and ultraviolet conditions to obtain a bacterial cellulose-based hydrogel.
[0036] The obtained bacterial cellulose-based hydrogel product was subjected to performance tests as follows:
[0037] 1) Morphology test results
[0038] Figure 3 The confocal morphology image of the bacterial cellulose-based hydrogel prepared in the present invention shows that the synthetic bacterial cellulose-based hydrogel has a dense structure.
[0039] 2) Mechanical properties test results of materials
[0040] like Figure 4As shown, the bacterial cellulose-based hydrogel prepared in this example has excellent mechanical properties, and the tensile results show that the material has a maximum tensile strength of 6.75 MPa. Test conditions: The composite hydrogel sample is cut into rectangular strips (length 40 mm, width 5 mm, thickness 1 mm), and its two ends are clamped on the sample stage, the load is adjusted to zero, and then the mechanical properties of the hydrogel are tested at a tensile speed of 20 mm / min.
[0041] 3) Material adhesion performance test results
[0042] The bacterial cellulose-based hydrogel prepared in this example has excellent tissue adhesion properties, such as Figure 5 As shown, the maximum adhesion of the hydrogel to pig skin is 1.4N, indicating that the material has excellent tissue adhesion properties. Test conditions: The hydrogel is attached between two pieces of skin tissue to establish a lap shear joint (10mm×5mm). At room temperature, the two ends of the pig skin are clamped on the sample table, the load is adjusted to zero, and a longitudinal tensile shear test is performed on a universal testing machine (WDW-5) at a speed of 10mm / min.
[0043] 4) Test results of material antifreeze and moisture retention performance
[0044] Figure 6 As shown in FIG. 1 , the two hydrogels prepared by using pure water (i.e., replacing the glycerol / water mixed solution in step 2 with pure water) and glycerol / water as solvents were placed in a refrigerator at -20°C for 48 hours. The hydrogel of the glycerol / water system did not freeze, while the hydrogel prepared by pure water froze significantly. In addition, Figure 7 As shown, the hydrogel of the glycerol / water system has good moisturizing properties, with a water loss rate of only about 10%, while the hydrogel prepared with pure water has a large water loss rate of 42%.
[0045] 5) CCK-8 cell viability test
[0046] The hydrogel product obtained in Example 1 was prepared with sterile PBS buffer at concentrations of 0, 0.5, 1, and 2 mg / mL. The cultured mouse fibroblast cell line was seeded in a 96-well plate at a density of 8,000 cells / well with a volume of 100 μL per well. After overnight culture, the plate was washed with PBS 2-3 times, and then the above-mentioned materials of various concentrations were added and co-cultured with the cells for different time periods. PBS buffer was used as a blank control. After the culture was completed, the plate was washed with 100 μL PBS, and then 90 μL serum-free culture medium and 10 μL CCK-8 solution were added to each well, incubated at 37°C for 2-4 hours, and the absorbance at 450 nm was detected with an enzyme marker. The results of cell viability detection by CCK-8 method showed that the bacterial cellulose-based hydrogel did not show obvious cytotoxicity, such as Figure 8As shown, the test results show that within the range of 0-2 mg / mL, the cell activity is maintained above 87%.
[0047] Example 2
[0048] A method for preparing a bacterial cellulose-based hydrogel comprises the following steps:
[0049] (1) Preparation of N-acryloyl aspartic acid: Aspartic acid (8 g) and sodium hydroxide (7.2 g) were dissolved in 70 mL of deionized water, placed in an ice bath and stirred vigorously. Subsequently, 6.8 mL of acryloyl chloride and 15 mL of dimethyl sulfoxide were fully mixed and added dropwise to the above reaction system. During the reaction, the pH was maintained at 7-8. The reactants were further stirred at room temperature for 3-4 hours. Subsequently, the pH of the mixture was adjusted to 11 with 2 M NaOH, and then washed with a large amount of ethyl acetate to remove the organic phase. The pH of the aqueous phase was acidified to 2 with 4 M HCl, and then the aqueous phase was extracted again with a large amount of ethyl acetate. The organic layer was dried over magnesium sulfate, filtered, concentrated, and precipitated in n-hexane. The precipitation was repeated for further purification.
[0050] (2) Preparation of bacterial cellulose-based hydrogel: First, 200 mL of a bacterial cellulose solution with a mass fraction of 0.25% was filtered and compressed to prepare a bacterial cellulose film, and the film was dried. Then, 0.1 g of N-[tri(hydroxymethyl)methyl]acrylamide and 0.2 g of N-acryloyl aspartic acid were added to 1 mL of a glycerol / water mixed solution system, a crosslinking agent (0.03 mg) and an initiator (0.06 mg) were added, and the dried bacterial cellulose film was immersed in the above mixed solution. After a period of time, it was injected into a mold and irradiated for 15 minutes under oxygen-free and ultraviolet conditions to obtain a bacterial cellulose-based hydrogel.
[0051] The same method as in Example 1 was used to test the performance of the bacterial cellulose-based hydrogel prepared in this example. The results are as follows:
[0052] The maximum tensile strength is 4.32MPa
[0053] The maximum adhesion force to pig skin is 1.1N;
[0054] Water retention rate is 90%;
[0055] The cell viability was maintained at 95%.
[0056] Example 3
[0057] A method for preparing a bacterial cellulose-based hydrogel comprises the following steps:
[0058] (1) Preparation of N-acryloyl aspartic acid: Aspartic acid (10 g) and sodium hydroxide (9 g) were dissolved in 80 mL of deionized water, placed in an ice bath and stirred vigorously. Subsequently, 9 mL of acryloyl chloride and 19.3 mL of dimethylformamide were fully mixed and added dropwise to the above reaction system. During the reaction, the pH was maintained at 7-8. The reactants were further stirred at room temperature for 3-4 hours. Subsequently, the pH of the mixture was adjusted to 11 with 4 M NaOH, and then washed with a large amount of ethyl acetate to remove the organic phase. The pH of the aqueous phase was acidified to 2 with 6 M HCl, and then the aqueous phase was extracted again with a large amount of ethyl acetate. The organic layer was dried over magnesium sulfate, filtered, concentrated, and precipitated in n-hexane. The precipitation was repeated for further purification.
[0059] (2) Preparation of bacterial cellulose-based hydrogel: First, 200 mL of a bacterial cellulose solution with a mass fraction of 0.5% was filtered and compressed to prepare a bacterial cellulose film, and the film was dried. Then, 0.2 g of N-[tris(hydroxymethyl)methyl]acrylamide and 0.3 g of N-acryloyl aspartic acid were added to a 1 mL glycerol / water mixed solution system, a crosslinking agent (0.1 mg) and an initiator (0.15 mg) were added, and the dried bacterial cellulose film was immersed in the above mixed solution. After a period of time, it was injected into a mold and irradiated for 30 minutes under oxygen-free and ultraviolet conditions to obtain a bacterial cellulose-based hydrogel.
[0060] The same method as in Example 1 was used to test the performance of the bacterial cellulose-based hydrogel prepared in this example. The results are as follows:
[0061] The maximum tensile strength is 12.92MPa
[0062] The maximum adhesion to pig skin is 1.8N;
[0063] The water retention rate is 91%;
[0064] The cell viability was maintained at 82%.
[0065] The above embodiments are only used to illustrate the technical solutions of the present invention, and are not intended to limit the present invention. Any changes, substitutions, modifications, and simplifications made by ordinary technicians in this technical field within the essential scope of the present invention are equivalent transformations, do not depart from the purpose of the present invention, and should also fall within the scope of protection of the claims of the present invention.
Claims
1. A high-strength bacterial cellulose-based hydrogel with antifreeze and moisture retention, characterized in that: The raw materials include the following parts by weight: 5-10 parts of bacterial cellulose, 10-20 parts of N-[tris(hydroxymethyl)methyl]acrylamide (THMA), and 20-30 parts of N-acryloyl aspartic acid (AASP); The hydrogel is prepared by the following method: firstly preparing bacterial cellulose into a film by weight, then adding N-[tris(hydroxymethyl)methyl]acrylamide and N-acryloyl aspartic acid into a mixed solution system of glycerol and water, adding a crosslinking agent and an initiator, immersing the bacterial cellulose film in the above solution after fully dissolving, and polymerizing under ultraviolet light and oxygen-free conditions to obtain a high-strength bacterial cellulose-based hydrogel with antifreeze and moisture retention.
2. The high-strength bacterial cellulose-based hydrogel with antifreeze and moisture retention according to claim 1, characterized in that: The N-acryloyl aspartic acid is prepared by the following method: Aspartic acid and sodium hydroxide are dissolved in ice-cold deionized water in a mass ratio of 8-10:7-9 to obtain a solution, acryloyl chloride and a polar solvent are fully mixed in a volume ratio of 7-9:15-19, and added dropwise to the above solution. During the reaction, the pH is maintained at a weak alkaline state, and the reaction is further carried out at room temperature for 3-5 hours; The pH of the mixture was adjusted to alkaline conditions, the organic phase was removed by washing, the pH of the aqueous phase was adjusted to acidic conditions, and then the aqueous phase was extracted again, the organic layer was dried, filtered, concentrated, and precipitated in n-hexane, the precipitation was repeated for further purification, and the collected product was dried in vacuo.
3. The antifreeze and moisture-retaining high-strength bacterial cellulose-based hydrogel according to claim 2, characterized in that: The reaction condition of aspartic acid and sodium hydroxide is ice bath.
4. The antifreeze and moisture-retaining high-strength bacterial cellulose-based hydrogel according to claim 2, characterized in that: The polar solvent includes dimethyl sulfoxide, tetrahydrofuran or dimethylformamide.
5. The antifreeze and moisture-retaining high-strength bacterial cellulose-based hydrogel according to claim 2, characterized in that: The pH of the mixture is adjusted to alkaline with NaOH, the concentration of NaOH is 2-5 M; The pH of the aqueous phase is adjusted to acidic using HCl, and the concentration of HCl is 3-6 M; Ethyl acetate was used for washing and extraction.
6. A method for preparing the high-strength bacterial cellulose-based hydrogel with antifreeze and moisture retention as claimed in claim 1, characterized in that: The following steps are involved: The hydrogel comprises the following raw materials in parts by weight: 5-10 parts of bacterial cellulose, 10-20 parts of N-[tris(hydroxymethyl)methyl]acrylamide (THMA), and 20-30 parts of N-acryloyl aspartic acid (AASP); the bacterial cellulose is first prepared into a film by weight, and then N-[tris(hydroxymethyl)methyl]acrylamide and N-acryloyl aspartic acid are added to a mixed solution system of glycerol and water, and a cross-linking agent and an initiator are added. After fully dissolved, the bacterial cellulose film is immersed in the above solution, and polymerized under ultraviolet light and anaerobic conditions to obtain a high-strength bacterial cellulose-based hydrogel with antifreeze and moisture retention.
7. The method for preparing the high-strength bacterial cellulose-based hydrogel with antifreeze and moisture retention according to claim 6, characterized in that: Based on the total mass of bacterial cellulose, N-[tris(hydroxymethyl)methyl]acrylamide and N-acryloyl aspartic acid as 100, the mass percentage of the crosslinking agent is 0.01-0.02%, and the mass percentage of the initiator is 0.02-0.03%.
8. The method for preparing the high-strength bacterial cellulose-based hydrogel with antifreeze and moisture retention according to claim 6, characterized in that: The crosslinking agent is one or more of polyethylene glycol diacrylate, N,N-methylenebisacrylamide, cyclotriene bond, and triallyl isocyanurate.
9. The method for preparing the high-strength bacterial cellulose-based hydrogel with antifreeze and moisture retention according to claim 6, characterized in that: The initiator is one or more of 2-hydroxy-2-methylpropiophenone, ammonium persulfate and α-ketoglutaric acid.
Citation Information
Patent Citations
Hydrogel tissue adhesive based on dicarboxyl amino acid and preparation method thereof
CN115612009A