A proton-electron mixed conductor material suitable for perovskite ceramic hydrogen separation membrane and a preparation method thereof

By doping CeO2 into perovskite ceramic hydrogen separation membrane to construct proton-electron hybrid conductor materials, the problems of unstable metal materials in the prior art under reduced atmosphere and low proton conductivity are solved, and more efficient Hydrogen separation performance.

CN116246814BActive Publication Date: 2024-11-29SHANGHAI INSTITUTE OF APPLIED PHYSICS CHINESE ACADEMY OF SCIENCES
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202211604748.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-13
Publication Date
2024-11-29
Estimated Expiration
2042-12-13

AI Technical Summary

Technical Problem

In the existing perovskite ceramic hydrogen separation membrane, metal materials doped in a reducing atmosphere are unstable, and the proton conductivity is low, making it difficult to meet the needs of efficient hydrogen separation.

Method used

Design a proton-electron hybrid conductor material with the chemical formula (1-x)BaZr0.1Ce0.7Y0.1Yb0.1O3-δ-xCeO2, by doping CeO2 into the conventional BaZr0.1Ce0.7Y0.1Yb0.1O3-δ , construct hybrid conductor materials to improve conductivity.

Benefits of technology

This material has certain electron conduction properties at high temperatures, which significantly improves the hydrogen permeability of the hydrogen separation membrane, solves the problems of unstable and low proton conductivity of traditional materials under reducing atmospheres, and provides a more stable hydrogen separation membrane Material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116246814B_ABST
    Figure CN116246814B_ABST
Patent Text Reader

Abstract

This invention relates to the field of materials preparation, and in particular to a proton-electron hybrid conductor material suitable for perovskite ceramic hydrogen separation membranes and its preparation method. The chemical formula of the proton-electron hybrid conductor material is: (1-x)BaZr a Ce b Y c Yb d O 3‑δ -xCeO2, wherein x is selected from 0.1 to 0.5, and a+b+c+d=1. This invention has the expected elemental distribution and atomic ratio, and due to the electronic conductivity of Ce ions at high temperatures, it can achieve high hydrogen separation performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of material preparation, and in particular to a proton-electron mixed conductor material suitable for a perovskite ceramic hydrogen separation membrane and a preparation method thereof. Background Art

[0002] Energy is the driving force for social progress. Hydrogen energy has the advantages of no pollution and high combustion calorific value, and has gradually become the most promising part of renewable energy. It has gradually attracted people's attention. However, in addition to hydrogen, the tail gas of large-scale industrial hydrogen production often contains other impurity gases, which may poison equipment and threaten human health. Therefore, purifying hydrogen has become an indispensable step in industrial hydrogen production. Dense hydrogen separation membrane technology, due to its low price, high efficiency and low energy consumption, is gradually becoming a research hotspot in hydrogen separation technology.

[0003] Traditional proton conductor material BaZr 0.1 Ce 0.7 Y 0.1 Yb 0.1 0 3-δ (BZCYYb) has attracted much attention due to its high proton conductivity. In perovskite ceramic hydrogen separation membrane materials, the method of constructing an electronic conductive phase by doping metal elements into BZCYYb is attracting the attention of many scholars.

[0004] In order to further improve the performance of perovskite ceramic hydrogen permeable membranes and solve the current problems of instability of metal materials under reducing atmosphere and low proton conductivity, the present invention designs a method of doping BZCYYb with CeO2 to construct a proton-electron mixed conductor material for perovskite ceramic hydrogen separation membranes. Summary of the invention

[0005] In view of the above-mentioned shortcomings of the prior art, the purpose of the present invention is to provide a proton-electron mixed conductor material suitable for perovskite ceramic hydrogen separation membrane and a preparation method thereof, so as to solve the problems in the prior art that metal materials doped in a reducing atmosphere are unstable and have low proton conductivity.

[0006] To achieve the above-mentioned and other related purposes, one aspect of the present invention provides a proton-electron mixed conductor material, wherein the chemical formula of the proton-electron mixed conductor material is:

[0007] (1-x)BaZr a Ce b Y c Yb d O 3-δ -xCeO2, wherein the x is selected from 0.1 to 0.5; a+b+c+d=1; and the δ is selected from 0 to 0.5.

[0008] In some embodiments of the present invention, the chemical formula of the proton-electron mixed conductor material is: (1-x)BaZr 0.1 Ce 0.7 Y 0.1 Yb 0.1 O 3-δ -xCeO2, wherein the x is selected from 0.1 to 0.5, and the δ is selected from 0 to 0.5.

[0009] In some embodiments of the present invention, in the chemical formula of the proton-electron mixed conductor material, x is selected from 0.3 to 0.5; preferably, x is selected from 0.3 or 0.5.

[0010] Another aspect of the present invention provides a method for preparing the proton-electron mixed conductor material according to the first aspect of the present invention, comprising: providing a precursor of the proton-electron mixed conductor material, and forming the proton-electron mixed conductor material by sintering the precursor.

[0011] In some embodiments of the present invention, the method for preparing the precursor comprises:

[0012] 1) dissolving barium salt, zirconium salt, yttrium salt, ytterbium salt and cerium salt in a solvent, mixing with a complexing agent, adjusting the pH value of the solution with a pH adjusting agent, and then heating and stirring the solution;

[0013] 2) heating the solution obtained in step 1) and drying it to obtain a precursor.

[0014] In some embodiments of the present invention, in step 1), the barium salt is selected from barium nitrate.

[0015] In some embodiments of the present invention, in step 1), the zirconium salt is selected from zirconium nitrate.

[0016] In some embodiments of the present invention, in step 1), the yttrium salt is selected from yttrium nitrate.

[0017] In some embodiments of the present invention, in step 1), the ytterbium salt is selected from ytterbium nitrate.

[0018] In some embodiments of the present invention, in step 1), the cerium salt is selected from cerium nitrate.

[0019] In some embodiments of the present invention, in step 1), the solvent is selected from water, preferably deionized water.

[0020] In some embodiments of the present invention, in step 1), the complexing agent is selected from citric acid and / or ethylenediaminetetraacetic acid; preferably, the molar ratio of the sum of metal ions in barium salts, zirconium salts, yttrium salts, ytterbium salts, and cerium salts to citric acid and ethylenediaminetetraacetic acid is 0.5-2:0.5-2:0.5-2.

[0021] In some embodiments of the present invention, in step 1), the pH adjuster is selected from aqueous ammonia, and the pH value is adjusted to 6-9.

[0022] In some embodiments of the present invention, in step 1), the heating temperature for stirring is 70-100°C.

[0023] In some embodiments of the present invention, in step 2), the heating temperature is 70°C to 100°C.

[0024] In some embodiments of the present invention, the sintering temperature is 800-1150°C.

[0025] In some embodiments of the present invention, sintering is performed in an air atmosphere.

[0026] In some embodiments of the present invention, the sintering time is 5 to 20 hours.

[0027] Another aspect of the present invention provides use of the proton-electron mixed conductor material according to the present invention in a perovskite ceramic hydrogen separation membrane.

[0028] Another aspect of the present invention provides a perovskite ceramic hydrogen separation membrane, comprising the proton-electron mixed conductor material as described in the first aspect of the present invention.

[0029] Another aspect of the present invention provides a method for preparing the aforementioned perovskite ceramic hydrogen separation membrane of the present invention, comprising tableting a powder of a proton-electron mixed conductor material, and sintering to obtain a perovskite ceramic hydrogen separation membrane; preferably, the sintering temperature is 1200-1500°C. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 The 70 mol% BaZr 0.1 Ce 0.7 Y 0.1 Yb 0.1 0 3-δ -XRD pattern of 30mol% CeO2 material.

[0031] Figure 2 The 70 mol% BaZr 0.1 Ce 0.7 Y 0.1 Yb 0.1 0 3-δ -Scanning electron microscope (SEM) image of 30mol% CeO2 powder.

[0032] Figure 3 The 70 mol% BaZr 0.1 Ce0.7 Y 0.1 Yb 0.1 0 3-δ -Energy distribution spectrum (EDS) image of different elements in 30mol% CeO2 powder.

[0033] Figure 4 The 50 mol% BaZr described in Example 2 of the present invention 0.1 Ce 0.7 Y 0.1 Yb 0.1 0 3-δ -XRD pattern of 50mol% CeO2 material.

[0034] Figure 5 The 50 mol% BaZr described in Example 2 of the present invention 0.1 Ce 0.7 Y 0.1 Yb 0.1 0 3-δ -Scanning electron microscope (SEM) image of 50mol% CeO2 powder.

[0035] Figure 6 The 50 mol% BaZr described in Example 2 of the present invention 0.1 Ce 0.7 Y 0.1 Yb 0.1 0 3-δ -Energy distribution spectrum (EDS) images of different elements in 50mol% CeO2 powder.

[0036] Figure 7 The 50 mol% BaZr described in Example 2 of the present invention 0.1 Ce 0.7 Y 0.1 Yb 0.1 0 3-δ -Hydrogen permeability graph of 50mol% CeO2 in 10%H2-90%He atmosphere at 700℃.

[0037] Figure 8 The 70 mol% BaZr 0.09 Ce 0.63 Y 0.09 Yb 0.09 Ni 0.1 0 3-δ -Scanning electron microscope (SEM) image of 30mol% CeO2 powder.

[0038] Fig. 9 The 70 mol% BaZr 0.09Ce 0.63 Y 0.09 Yb 0.09 Ni 0.1 0 3-δ -Energy distribution spectrum (EDS) image of different elements in 30mol% CeO2 powder.

[0039] Fig.10 This is the hydrogen permeability of Example 4 of the present invention.

[0040] Fig.11 This is the hydrogen permeability of Example 5 of the present invention. DETAILED DESCRIPTION

[0041] The following is a detailed description of an embodiment of a proton-electron mixed conductor material and a preparation method thereof of the present application.

[0042] "Scope" disclosed in the present application is limited in the form of lower limit and upper limit, and a given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of a special range. The scope limited in this way can be including end values ​​or not including end values, and can be arbitrarily combined, that is, any lower limit can be combined with any upper limit to form a scope. For example, if the scope of 60-120 and 80-110 is listed for a specific parameter, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range values ​​1 and 2 are listed, and if the maximum range values ​​3, 4 and 5 are listed, the following scope can be all expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In the present application, unless otherwise specified, the numerical range "ab" represents the abbreviation of any real number combination between a and b, wherein a and b are real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" are listed in this document, and "0-5" is just an abbreviation of these numerical combinations. In addition, when a parameter is expressed as an integer ≥ 2, it is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.

[0043] After a lot of exploration and experiments, the inventors of the present invention have provided a proton-electron mixed conductor material suitable for perovskite ceramic hydrogen separation membrane and its preparation method. 0.1 Ce 0.7 Y 0.1 Yb 0.1 0 3-δ The hybrid proton-electron conductor material is constructed, which has certain electronic conductivity at high temperature and can be used as a perovskite ceramic hydrogen separation membrane material. On this basis, the present invention is completed.

[0044] The first aspect of the present invention provides a proton-electron mixed conductor material, wherein the chemical formula of the proton-electron mixed conductor material is: (1-x)BaZr a Ce b Y c Yb d O 3-δ -xCeO2, wherein the x is selected from 0.1 to 0.5; a+b+c+d=1; and the δ is selected from 0 to 0.5.

[0045] In the proton-electron mixed conductor material provided by the present invention, preferably, the chemical formula of the proton-electron mixed conductor material is: (1-x)BaZr 0.1 Ce 0.7 Y 0.1 Yb 0.1 O 3-δ -xCeO2, wherein the x is selected from 0.1 to 0.5, and the δ is selected from 0 to 0.5.

[0046] In the proton-electron mixed conductor material provided by the present invention, x=0.1-0.3, or x=0.3-0.5, etc. Preferably, x is selected from 0.3 or 0.5. For better description, in the present invention, when x=0.3, the proton-electron mixed conductor material can be recorded as 70 mol% BaZr 0.1 Ce 0.7 Y 0.1 Yb 0.1 0 3-δ -30mol% CeO2. When x = 0.5, the proton-electron mixed conductor material can be recorded as 50mol% BaZr 0.1 Ce 0.7 Y 0.1 Yb 0.1 0 3-δ -50mol%CeO2.

[0047] In the proton-electron mixed conductor material provided by the present invention, δ is selected from 0 to 0.5, 0 to 0.1, 0.1 to 0.2, 0.2 to 0.3, 0.3 to 0.4, or 0.4 to 0.5.

[0048] The second aspect of the present invention provides a method for preparing a proton-electron mixed conductor material, the method comprising: providing a precursor of the proton-electron mixed conductor material, and forming the proton-electron mixed conductor material by sintering the precursor.

[0049] In the method for preparing the proton-electron mixed conductor material provided by the present invention, the method for preparing the precursor comprises:

[0050] 1) dissolving barium salt, zirconium salt, yttrium salt, ytterbium salt and cerium salt in a solvent, mixing with a complexing agent, adjusting the pH value of the solution with a pH adjusting agent, and then heating and stirring the solution;

[0051] 2) heating the solution obtained in step 1) and drying it to obtain a precursor.

[0052] In the preparation method of the precursor of the present invention, step 1) is to dissolve the barium salt, zirconium salt, yttrium salt, ytterbium salt and cerium salt in a solvent, mix with a complexing agent, and heat and stir the solution after adjusting the pH value of the solution by a pH adjusting agent. Among them, the cerium salt is excessive. In step 1) of the present invention, the barium salt is selected from barium nitrate. The zirconium salt is selected from zirconium nitrate. The yttrium salt is selected from yttrium nitrate. The ytterbium salt is selected from ytterbium nitrate. The cerium salt is selected from cerium nitrate.

[0053] In step 1) of the present invention, the solvent is selected from water, preferably deionized water. Barium nitrate, zirconium nitrate, yttrium nitrate, ytterbium nitrate and excess cerium nitrate are dissolved in deionized water, heated and stirred to form a clear solution.

[0054] In step 1) of the present invention, the complexing agent is selected from citric acid and / or ethylenediaminetetraacetic acid. Preferably, the complexing agent is selected from citric acid and ethylenediaminetetraacetic acid.

[0055] In step 1) of the present invention, the molar ratio of the sum of metal ions in barium salt, zirconium salt, yttrium salt, ytterbium salt and cerium salt to citric acid and ethylenediaminetetraacetic acid is 0.5-2:0.5-2:0.5-2.

[0056] In step 1) of the present invention, the pH adjusting agent is selected from ammonia water, and the pH value is adjusted to 6-9, 6-7, 7-8, or 8-9.

[0057] The heating temperature for stirring in step 1) of the present invention can be, for example, 70°C to 100°C, 70°C to 80°C, 80°C to 90°C, or 90°C to 100°C.

[0058] In the method for preparing the precursor of the present invention, step 2) is to heat the solution obtained in step 1) and dry it to obtain the precursor. Specifically, when most of the water in the solution evaporates to form a gel, the obtained gel is dried to obtain a black and fluffy proton-electron mixed conductor precursor. The drying is performed in a blast drying oven, for example.

[0059] In step 2), the heating temperature can be, for example, 70°C to 100°C, 70°C to 80°C, 80°C to 90°C, or 90°C to 100°C. The stirring time can be, for example, 2 to 5 hours. The heating time is preferably 100°C, and the stirring time is controlled to be 3 hours.

[0060] In the preparation method of the proton-electron mixed conductor material of the present invention, in the step of forming the proton-electron mixed conductor material by sintering the precursor, the sintering temperature can be, for example, 800-1150° C., 800-900° C., 900-1000° C., or 1000-1150° C., etc. The sintering time can be, for example, 5-20 hours, 5-10 hours, 5-8 hours, 8-10 hours, or 10-20 hours, etc. The sintering can be, for example, calcined in a muffle furnace. And the sintering is performed in an air atmosphere.

[0061] The third aspect of the present invention provides use of the proton-electron mixed conductor material as described above in a perovskite ceramic hydrogen separation membrane.

[0062] The fourth aspect of the present invention provides a perovskite ceramic hydrogen separation membrane, comprising the proton-electron mixed conductor material as described in the first aspect of the present invention.

[0063] The fifth aspect of the present invention provides a method for preparing the aforementioned perovskite ceramic hydrogen separation membrane, comprising pressing a powder of a proton-electron mixed conductor material into a tablet, and sintering the tablet to obtain a perovskite ceramic hydrogen separation membrane. Specifically, the obtained powder is pressed into a tablet, placed in a muffle furnace for sintering, and then polished on both sides to obtain a perovskite ceramic hydrogen separation membrane sample.

[0064] In the preparation method of the perovskite ceramic hydrogen separation membrane provided by the present invention, the sintering temperature can be 1200-1500°C, 1200-1300°C, 1300-1400°C, or 1400-1500°C. The sintering time can be, for example, 5-20 hours. In one embodiment, the sintering temperature is set to 1400°C and the holding time is set to 5 hours.

[0065] The beneficial effects of the present invention are:

[0066] The chemical formula of the material of the present invention is (1-x)BaZr a Ce b Y c Yb d O 3-δ -xCeO2, the first disclosure and preparation of excess Ce element doped BaZr a Ce b Y c Yb d O 3-δ -xCeO2 (e.g. BaZr 0.1 Ce 0.7 Y 0.1 Yb 0.1 0 3-δ) constructs a hybrid proton-electron conductor material, which has certain electronic conductivity at high temperature and can be used as a perovskite ceramic hydrogen separation membrane material. The hydrogen permeability of the hydrogen separation membrane at the working temperature is greatly improved compared with the traditional proton conductor, which can provide more options for the stable operation and commercial application of hydrogen separation membrane materials; in addition, the sol-gel method is used to prepare (1-x)BaZr doped with excessive Ce element a Ce b Y c Yb d O 3-δ -xCeO2 material meets the expected elemental composition, which is conducive to the on-demand regulation of element ratios.

[0067] The following describes the embodiments of the present invention through specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention.

[0068] In the following examples, the reagents, materials and instruments used are all commercially available unless otherwise specified.

[0069] Example 1

[0070] Proton-electron mixed conductor material 70mol%BaZr 0.1 Ce 0.7 Y 0.1 Yb 0.1 0 3-δ Preparation of -30mol% CeO2

[0071] According to the chemical formula 70 mol% BaZr 0.1 Ce 0.7 Y 0.1 Yb 0.1 0 3-δ -30mol% CeO2 preparation product 0.01mol, weigh the metal nitrates in the corresponding stoichiometric ratio, specifically 1.8293g barium nitrate, 0.3005g zirconium nitrate pentahydrate, 3.4303g cerium nitrate hexahydrate, 0.2681g yttrium nitrate hexahydrate, 0.3144g ytterbium nitrate pentahydrate, add into a beaker filled with 300mL deionized water, stir with a magnetic stirrer, and heat until completely dissolved.

[0072] According to the molar ratio of ethylenediaminetetraacetic acid: citric acid: metal ion = 1:1:1, 9.9365 g of ethylenediaminetetraacetic acid and 7.1446 g of citric acid were weighed and added to the nitrate solution, and ammonia water was continuously added to adjust the pH to obtain a light yellow transparent sol solution.

[0073] Stir at 100°C until the water is completely evaporated to form a viscous colloid; put it into a blast drying oven to decompose the citric acid by heat, and the viscous colloid will turn into a mushroom cloud-like black fluffy powder.

[0074] The black fluffy powder was placed in a crucible, placed in a muffle furnace and sintered at 1000°C for 5 hours, and then taken out after cooling to obtain a proton-electron mixed conductor 70 mol% BaZr 0.1 Ce 0.7 Y 0.1 Yb 0.1 0 3-δ -30mol% CeO2 material powder.

[0075] 70mol%BaZr 0.1 Ce 0.7 Y 0.1 Yb 0.1 0 3-δ -30mol% CeO2 powder XRD spectrum as shown Figure 1 As shown, the analysis was performed using a German Bruker D8 Advance diffractometer with a scanning angle range of 2θ=20-80°, a scanning speed of 5° / min, and a scanning step length of 0.015°. Figure 1 It can be seen that the product is mainly BaZr 0.1 Ce 0.7 Y 0.1 Yb 0.1 0 3-δ phase and CeO2 phase, no other phases were found.

[0076] 70mol%BaZr 0.1 Ce 0.7 Y 0.1 Yb 0.1 0 3-δ The particle morphology and element distribution of -30mol% CeO2 powder are as follows Figure 2 and Figure 3 As shown, observation was performed using a German Zeiss, Cross Beam 540 scanning electron microscope. From the figure, it can be seen that the mixed proton-electron conductive material powder of the present invention has complete grains, and all elements are evenly distributed and the atomic ratio is in line with expectations.

[0077] Example 2

[0078] Proton-electron mixed conductor material 50mol%BaZr 0.1 Ce 0.7 Y 0.1 Yb 0.1 0 3-δ -Preparation of 50mol% CeO2

[0079] According to the chemical formula 50 mol% BaZr 0.1 Ce 0.7 Y 0.1 Yb 0.1 0 3-δ -50mol% CeO2 preparation product 0.01mol, weigh the metal nitrates in the corresponding stoichiometric ratio, specifically 1.3067g barium nitrate, 0.2146g zirconium nitrate pentahydrate, 3.6908g cerium nitrate hexahydrate, 0.1915g yttrium nitrate hexahydrate, 0.2246g ytterbium nitrate pentahydrate, add into a beaker filled with 300mL deionized water, stir with a magnetic stirrer, and heat until completely dissolved.

[0080] According to the molar ratio of ethylenediaminetetraacetic acid: citric acid: metal ion = 1:1:1, 8.7675 g of ethylenediaminetetraacetic acid and 6.3041 g of citric acid were weighed and added to the nitrate solution, and ammonia water was continuously added to adjust the pH to obtain a light yellow transparent sol solution.

[0081] Stir at 100°C until the water is completely evaporated to form a viscous colloid; put it into a blast drying oven to decompose the citric acid by heat, and the viscous colloid will turn into a mushroom cloud-like black fluffy powder.

[0082] The black fluffy powder was placed in a crucible, placed in a muffle furnace and sintered at 1000°C for 5 hours, and then taken out after cooling to obtain a proton-electron mixed conductor 50 mol% BaZr 0.1 Ce 0.7 Y 0.1 Yb 0.1 0 3-δ -50mol% CeO2 material powder.

[0083] 50mol%BaZr 0.1 Ce 0.7 Y 0.1 Yb 0.1 0 3-δ -50mol% CeO2 powder XRD spectrum Figure 4 As shown, the analysis was performed using a German Bruker D8 Advance diffractometer with a scanning angle range of 2θ=20-80°, a scanning speed of 5° / min, and a scanning step length of 0.015°. Figure 4 It can be seen that the product is mainly BaZr 0.1 Ce 0.7 Y 0.1 Yb 0.1 0 3-δ phase and CeO2 phase, no other phases were found.

[0084] 50mol%BaZr0.1 Ce 0.7 Y 0.1 Yb 0.1 0 3-δ The particle morphology and element distribution of -50mol% CeO2 powder are as follows Figure 5 and Figure 6 As shown, observation was performed using a German Zeiss, Cross Beam 540 scanning electron microscope. From the figure, it can be seen that the proton-electron hybrid conductive material powder of the present invention has complete grains, and all elements are evenly distributed and the atomic ratio is in line with expectations.

[0085] Example 3

[0086] Proton-electron mixed conductor material 70mol%BaZr 0.09 Ce 0.63 Y 0.09 Yb 0.09 Ni 0.1 0 3-δ Preparation of -30mol% CeO2

[0087] According to the chemical formula 70 mol% BaZr 0.09 Ce 0.63 Y 0.09 Yb 0.09 Ni 0.1 0 3-δ -30mol% CeO2 preparation product 0.01mol, weigh the metal nitrates in the corresponding stoichiometric ratio, specifically 1.8293g barium nitrate, 0.2704g zirconium nitrate pentahydrate, 3.2175g cerium nitrate hexahydrate, 0.2413g yttrium nitrate hexahydrate, 0.2830g ytterbium nitrate pentahydrate, 0.2036g nickel nitrate, add them into a beaker filled with 300mL deionized water, stir with a magnetic stirrer, and heat until completely dissolved.

[0088] According to the molar ratio of ethylenediaminetetraacetic acid: citric acid: metal ion = 1:1:1, 9.9365 g of ethylenediaminetetraacetic acid and 7.1446 g of citric acid were weighed and added to the nitrate solution, and ammonia water was continuously added to adjust the pH to obtain a light yellow transparent sol solution.

[0089] Stir at 100°C until the water is completely evaporated to form a viscous colloid; put it into a blast drying oven to decompose the citric acid by heat, and the viscous colloid will turn into a mushroom cloud-like black fluffy powder.

[0090] The black fluffy powder was placed in a crucible, placed in a muffle furnace and sintered at 1000°C for 5 hours, and then taken out after cooling to obtain a proton-electron mixed conductor 70 mol% BaZr 0.09 Ce 0.63 Y0.09 Yb 0.09 Ni 0.1 0 3-δ -30mol% CeO2 material powder.

[0091] 70mol%BaZr 0.09 Ce 0.63 Y 0.09 Yb 0.09 Ni 0.1 0 3-δ -30mol% CeO2 powder XRD spectrum as shown Figure 7 As shown, the analysis was performed using a German Bruker D8 Advance diffractometer with a scanning angle range of 2θ=20-80°, a scanning speed of 5° / min, and a scanning step length of 0.015°. Figure 7 It can be seen that the product is mainly BaZr 0.09 Ce 0.63 Y 0.09 Yb 0.09 Ni 0.1 0 3-δ phase and CeO2 phase, no other phases were found.

[0092] 70mol%BaZr 0.09 Ce 0.63 Y 0.09 Yb 0.09 Ni 0.1 0 3-δ The particle morphology and element distribution of -30mol% CeO2 powder are as follows Figure 8 and Fig. 9 As shown, the observation was carried out using a German Zeiss Cross Beam 540 scanning electron microscope. From the figure, it can be seen that the mixed proton-electron conductive material powder of the present invention has complete grains, and all elements are evenly distributed.

[0093] Example 4

[0094] Preparation of perovskite ceramic hydrogen separation membrane and hydrogen separation performance test

[0095] Utilize 50mol%BaZr 0.1 Ce 0.7 Y 0.1 Yb 0.1 0 3-δ -50mol% CeO2 material was pressed and sintered at a temperature of 1400℃ and a holding time of 10 hours to prepare a perovskite ceramic hydrogen separation membrane. The feed side was 10% H2-90% He, the purge was pure N2 atmosphere, and the temperature was 700℃ for testing. The hydrogen permeability was as follows Fig.10 shown.

[0096] Example 5

[0097] Preparation of perovskite ceramic hydrogen separation membrane and hydrogen separation performance test

[0098] Utilize 70mol%BaZr 0.09 Ce 0.63 Y 0.09 Yb 0.09 Ni 0.1 0 3-δ -30mol% CeO2 material was pressed and sintered at a temperature of 1300℃ and a holding time of 10 hours to prepare a perovskite ceramic hydrogen separation membrane. The feed side was 10% H2-90% He, the purge was pure N2 atmosphere, and the temperature was 700℃ for testing. The hydrogen permeability was as follows Fig.11 shown.

[0099] The above is only a preferred embodiment of the present invention and is not intended to limit the scope of the present invention. The above embodiments of the present invention can also be changed in various ways, the difference lies in the material composition. That is, all simple, equivalent changes and modifications made according to the claims of the present invention, i.e. the contents of the specification, fall within the scope of protection of the claims of this patent. The contents not described in detail in the present invention are all conventional technical contents.

Claims

1. A proton-electron mixed conductor material, wherein the chemical formula of the proton-electron mixed conductor material is: (1-x) BaZr a Ce b Y c Yb d O 3-δ -xCeO2, where The x is selected from 0.1 to 0.5; a+b+c+d=1; and the δ is selected from 0 to 0.

5.

2. The proton-electron mixed conductor material according to claim 1, characterized in that: The chemical formula of the proton-electron mixed conductor material is: (1-x) BaZr 0.1 Ce 0.7 Y 0.1 Yb 0.1 O 3-δ -xCeO2, wherein the x is selected from 0.1 to 0.5, and the δ is selected from 0 to 0.

5.

3. The proton-electron mixed conductor material according to claim 1, characterized in that: In the chemical formula of the proton-electron mixed conductor material, x is selected from 0.3 to 0.

5.

4. The proton-electron mixed conductor material according to claim 1, characterized in that: x is selected from 0.3 or 0.

5.

5. The method for preparing the proton-electron mixed conductor material according to any one of claims 1 to 4, comprising: A precursor of a proton-electron mixed conductor material is provided, and the proton-electron mixed conductor material is formed by sintering the precursor.

6. The method for preparing a proton-electron mixed conductor material according to claim 5, characterized in that: The preparation method of the precursor comprises: 1) dissolving barium salt, zirconium salt, yttrium salt, ytterbium salt and cerium salt in a solvent, mixing with a complexing agent, adjusting the pH value of the solution with a pH adjusting agent, and then heating and stirring the solution; 2) Heating the solution obtained in step 1) and drying it to obtain a precursor.

7. The method for preparing a proton-electron mixed conductor material according to claim 6, characterized in that: In step 1), the barium salt is selected from barium nitrate; And / or, in step 1), the zirconium salt is selected from zirconium nitrate; And / or, in step 1), the yttrium salt is selected from yttrium nitrate; and / or, in step 1), the ytterbium salt is selected from ytterbium nitrate; And / or, in step 1), the cerium salt is selected from cerium nitrate; And / or, in step 1), the solvent is selected from water; And / or, in step 1), the complexing agent is selected from citric acid and / or ethylenediaminetetraacetic acid; And / or, in step 1), the pH adjusting agent is selected from aqueous ammonia, and the pH value is adjusted to 6-9; And / or, in step 1), the stirring heating temperature is 70-100°C; And / or, in step 2), the heating temperature is 70°C to 100°C.

8. The method for preparing a proton-electron mixed conductor material according to claim 7, characterized in that: The solvent is deionized water.

9. The method for preparing a proton-electron mixed conductor material according to claim 7, characterized in that: The molar ratio of the sum of metal ions in barium salt, zirconium salt, yttrium salt, ytterbium salt and cerium salt to citric acid and ethylenediaminetetraacetic acid is 0.5~2:0.5~2:0.5~2.

10. The method for preparing a proton-electron mixed conductor material according to claim 5, characterized in that: The sintering temperature is 800~1150℃; and / or, sintering in an air atmosphere; And / or, the sintering time is 5 to 20 hours.

11. Use of the proton-electron mixed conductor material according to any one of claims 1 to 4 in a perovskite ceramic hydrogen separation membrane.

12. A perovskite ceramic hydrogen separation membrane, comprising the proton-electron mixed conductor material according to any one of claims 1 to 4.

13. The method for preparing the perovskite ceramic hydrogen separation membrane according to claim 12, comprising pressing powder of the proton-electron mixed conductor material into tablets and sintering to obtain the perovskite ceramic hydrogen separation membrane.

14. The method for preparing a perovskite ceramic hydrogen separation membrane according to claim 13, characterized in that: The sintering temperature is 1200-1500°C.

Citation Information

Patent Citations

  • Method for preparing proton conductor ceramic by low-temperature densification

    CN102584222A

  • Anion-doped perovskite mixed conductor hydrogen permeation membrane material and preparation method and application thereof

    CN106925136A