A 3D / 2D ZnO / gC 3 N 4 Preparation method of nanocomposite photocatalytic material
By constructing a heterojunction structure between ZnO and g-C3N4 to form a 3D/2D ZnO/g-C3N4 nanocomposite, the problems of high cost and limited catalytic activity of existing photocatalytic materials in water pollution treatment are solved. The efficient degradation effect of tetracycline is achieved.
Patent Information
- Application Number
- CN202310323415.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2043-03-30
Smart Images

Figure CN116251613B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of inorganic materials, and specifically relates to a method for preparing a 3D / 2D ZnO / g-C3N4 nanocomposite photocatalytic material. Background Art
[0002] The rapid development of the chemical and pharmaceutical industries has brought a rich and convenient life to human beings. At the same time, the pollution caused by their irregular use has also brought many harms to people. Among them, water pollution, which is closely related to life, is directly or indirectly endangering human health. Therefore, it is particularly important to find ways to purify water pollution. To date, physical, microbiological and chemical methods are often used in industry to treat pollutants in wastewater. Among them, physical methods are often limited by material prices and repeated recycling, while microbiological methods are limited by pollutant concentrations. Large pollutant concentrations will lead to the death of microorganisms. In comparison, chemical methods have the advantages of being green, energy-saving and efficient. In the development of chemical methods, considering energy issues, researchers turned their attention to solar energy, which has abundant reserves, is easy to obtain and widely used on the earth, so semiconductor photocatalytic technology has gradually entered the field of vision of researchers.
[0003] In recent years, semiconductors such as metal oxides, metal sulfides, non-metallic two-dimensional materials, silver-based semiconductor materials and bismuth compounds have been developed for use as photocatalytic materials. Graphitic carbon nitride (g-C3N4) is a metal-free two-dimensional π-conjugated polymer with a layered structure similar to graphite. Its visible light absorption range of 450-460nm and excellent energy band structure make it a good semiconductor photocatalytic material that can well match the thermodynamic requirements of photoredox reactions. However, the inherent electronic structure of g-C3N4 itself limits its selection of a single type of pollutant for catalytic degradation, and it cannot be widely used. Therefore, it is necessary to develop heterojunctions with metal oxides to change the defects caused by its energy band structure, thereby improving its photocatalytic performance. Summary of the invention
[0004] In order to solve the above technical problems, the present invention provides a method for preparing a ZnO / g-C3N4 composite photocatalytic material with simple process and relatively low cost.
[0005] Zinc oxide (ZnO) is a wide bandgap (~3.3eV) n-type semiconductor commonly used in photocatalytic composite materials. It is easy to prepare and is green and safe. By comparing the band structures of ZnO and g-C3N4, it can be found that constructing a heterojunction structure between the two can effectively make up for their inherent defects. The present invention calcines the ZIF-8 precursor to stack ZnO to form a cubic porous structure, and adds g-C3N4 nanosheets during the calcination process so that it can be tightly coupled on the surface of cubic ZnO to form a heterojunction, thereby obtaining a ZnO / g-C3N4 composite photocatalytic material.
[0006] The present invention uses urea as a nitrogen-rich precursor to prepare g-C3N4 nanosheets, forms ZIF-8 on the surface of g-C3N4, and forms a ZnO / g-C3N4 heterojunction by high-temperature pyrolysis of ZIF-8 / g-C3N4. During the pyrolysis process, ZIF-8 provides a framework support for the formation of cubic porous ZnO, so that the g-C3N4 nanosheets are coupled to the surface of cubic ZnO, thereby increasing its specific surface area and light response range, providing more catalytic active sites, and finally preparing a nano-composite photocatalytic material with high photocatalytic performance.
[0007] The method for preparing a 3D / 2D ZnO / g-C3N4 nanocomposite photocatalytic material of the present invention comprises the following steps:
[0008] Step S1: Put urea into a crucible, place it in a muffle furnace for the first calcination to obtain a yellow block g-C3N4, grind the block g-C3N4 in an agate mortar to obtain a solid powder, and calcine the powder g-C3N4 for the second time to obtain g-C3N4 nanosheets;
[0009] Step S2: g-C3N4 nanosheets and 2-methylimidazole are mixed in a methanol solution, ultrasonically dispersed, and then rapidly stirred, and then zinc acetate / methanol solution is added, and stirred at room temperature to obtain ZIF-8 / g-C3N4;
[0010] Step S3: Place ZIF-8 / g-C3N4 in a muffle furnace, heat it from 20°C to 350°C and keep it at that temperature, then continue to heat it to 400°C and keep it at that temperature, and cool it to room temperature to obtain a ZnO / g-C3N4 nanocomposite photocatalytic material.
[0011] Furthermore, in the above technical solution, in step 1, the first calcination temperature is 550° C. for 4 hours, and the second calcination temperature is 500° C. for 4 hours.
[0012] Furthermore, in the above technical solution, in step 2, the ratio of g-C3N4 nanosheets to methanol is 8 mg / mL, and the molar ratio of zinc acetate to 2-methylimidazole is 1:4.
[0013] Furthermore, in the above technical solution, in step 3, a two-step calcination method is adopted, with a heating rate of 5°C / min from 20 to 350°C, a dwell time of 120min at 350°C, a heating rate of 2°C / min from 350 to 400°C, and a dwell time of 60min at 400°C.
[0014] Furthermore, in the above technical solution, the calcination gas atmosphere in step 1 and step 3 is air.
[0015] Furthermore, in the above technical solution, the specific steps of the preparation process are:
[0016] Step S1: 20 g of urea was placed in a 100 mL covered crucible, and then placed in a muffle furnace. The temperature of the muffle furnace was raised from room temperature to 550 ° C for 36 min and maintained for 4 h. After naturally cooling to room temperature, a yellow block of g-C3N4 was obtained. The block of g-C3N4 was ground to obtain a yellow solid powder. 300-500 mg of the powder was evenly spread on the bottom of a 100 mL covered crucible and placed in a muffle furnace. The temperature was raised to 500 ° C at a heating rate of 5 ° C / min and maintained for 4 h. After naturally cooling to room temperature, light yellow g-C3N4 nanosheets were obtained.
[0017] Step S2: 200 mg of g-C3N4 nanosheets and 3.28 g of 2-methylimidazole were mixed and dissolved in 25 mL of methanol solution, ultrasonicated for 30 min and then rapidly stirred for 2 h, and then 25 mL of zinc acetate solution / methanol (the mass of zinc acetate was 1.83 g) was added, and slowly stirred at room temperature for 24 h. The obtained solid methanol was centrifuged 5 times, placed in a drying oven and dried at 60 ° C for 8 h, and then ground to obtain ZIF-8 / g-C3N4;
[0018] Step S3: Put ZIF-8 / g-C3N4 into a covered crucible, place it in a muffle furnace, and heat it from room temperature to 350°C in air for 66 minutes and keep it for 120 minutes, then heat it to 400°C for 25 minutes and keep it for 60 minutes, and naturally cool it to room temperature to obtain a brown-yellow ZnO / g-C3N4 composite photocatalytic material.
[0019] The present invention uses the ZnO / g-C3N4 nanocomposite photocatalytic material prepared by the above method in the visible light catalytic degradation of tetracycline in water. The study found that the tetracycline removal rate was 87.57% within 40 minutes, and the degradation rate constant was 0.0440min -1 After 5 cycles, the removal rate still remained at 73.33%, showing excellent photocatalytic performance.
[0020] Beneficial effects of the present invention:
[0021] 1. The present invention uses ZIF-8 as a precursor to derive porous cubic ZnO under step-by-step high-temperature calcination, so that ZnO nanoparticles are orderly stacked and crystallized with ZIF-8 as a framework, avoiding the accumulation of ZnO to form large disordered clusters, which hinders its photochemical performance;
[0022] 2. The present invention uses g-C3N4 as a substrate and synthesizes ZIF-8 in situ on its surface. When the two are co-calcined, g-C3N4 is stably coated on the surface of cubic porous ZnO to form a tight heterojunction and enhance the photocatalytic performance of the composite material;
[0023] 3. The visible light response range of the ZnO / g-C3N4 composite material prepared by the present invention is greatly improved compared with that of a single component, and it is used in the degradation of tetracycline and has an excellent visible light catalytic decomposition effect. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 Transmission electron microscopy images of ZCN-2 prepared in Example 2 and ZnO prepared in Example 4;
[0025] Figure 2 Nitrogen adsorption-desorption isotherms for the preparation of CN and ZCN-2 in Example 2 and the preparation of ZnO in Example 4;
[0026] Figure 3 X-ray diffraction patterns for CN and ZCN-2 prepared in Example 2 and ZnO prepared in Example 4;
[0027] Figure 4 Fourier transform infrared spectra of CN and ZCN-2 prepared in Example 2 and ZnO prepared in Example 4;
[0028] Figure 5 X-ray photoelectron spectra of CN and ZCN-2 prepared in Example 2 and ZnO prepared in Example 4;
[0029] Figure 6 UV-visible diffuse reflectance spectra of CN and ZCN-2 prepared in Example 2 and ZnO prepared in Example 4;
[0030] Figure 7 Transient photocurrent response diagrams for CN and ZCN-2 prepared in Example 2 and ZnO prepared in Example 4;
[0031] Figure 8 Visible light photocatalytic degradation efficiency graphs of tetracycline prepared by CN, ZCN-1, ZCN-2, ZCN-3 and ZnO for Examples 1-4. DETAILED DESCRIPTION
[0032] The above contents of the present invention are further described in detail below through examples, but this should not be understood as the scope of the above subject matter of the present invention being limited to the following examples, and all technologies implemented based on the above contents of the present invention belong to the scope of the present invention.
[0033] Example 1
[0034] Step S1: 20 g of urea was placed in a 100 mL covered crucible, and then placed in a muffle furnace. The temperature of the muffle furnace was raised from room temperature to 550 ° C for 36 min and maintained for 4 h. After naturally cooling to room temperature, a yellow block of g-C3N4 was obtained. The block of g-C3N4 was ground to obtain a yellow solid powder. 300 mg of the powder was evenly spread on the bottom of a 100 mL covered crucible and placed in a muffle furnace. The temperature was raised to 500 ° C at a heating rate of 5 ° C / min and maintained for 4 h. After naturally cooling to room temperature, light yellow g-C3N4 nanosheets (CN) were obtained.
[0035] Step S2: 100 mg CN and 3.28 g 2-methylimidazole were mixed and dissolved in 25 mL methanol solution, ultrasonicated for 30 min and then rapidly stirred for 2 h, and then 25 mL methanol zinc acetate solution (the mass of zinc acetate was 1.83 g) was added, and slowly stirred at room temperature for 24 h. The obtained solid methanol was centrifuged 5 times, placed in a drying oven and dried at 60 ° C for 8 h, and then ground to obtain ZIF-8 / g-C3N4;
[0036] Step S3: Put ZIF-8 / g-C3N4 into a covered crucible, place it in a muffle furnace, and in air, heat it from room temperature to 350°C over 66 minutes and keep it for 120 minutes, then heat it to 400°C over 25 minutes and keep it for 60 minutes, and naturally cool it to room temperature to obtain a brown ZnO / g-C3N4 composite photocatalytic material (ZCN-1).
[0037] Example 2
[0038] Step S1: 20 g of urea was placed in a 100 mL covered crucible, and then placed in a muffle furnace. The temperature of the muffle furnace was raised from room temperature to 550 ° C for 36 min and maintained for 4 h. After naturally cooling to room temperature, a yellow block of g-C3N4 was obtained. The block of g-C3N4 was ground to obtain a yellow solid powder. 300 mg of the powder was evenly spread on the bottom of a 100 mL covered crucible and placed in a muffle furnace. The temperature was raised to 500 ° C at a heating rate of 5 ° C / min and maintained for 4 h. After naturally cooling to room temperature, light yellow g-C3N4 nanosheets (CN) were obtained.
[0039] Step S2: 200 mg CN and 3.28 g 2-methylimidazole were mixed and dissolved in 25 mL methanol solution, ultrasonicated for 30 min and then rapidly stirred for 2 h, and then 25 mL methanol zinc acetate solution (the mass of zinc acetate was 1.83 g) was added, and slowly stirred at room temperature for 24 h. The obtained solid methanol was centrifuged 5 times, placed in a drying oven and dried at 60 ° C for 8 h, and then ground to obtain ZIF-8 / g-C3N4;
[0040] Step S3: Put ZIF-8 / g-C3N4 into a crucible with a lid, place it in a muffle furnace, and in air, heat it from room temperature to 350°C over 66 minutes and keep it for 120 minutes, then heat it to 400°C over 25 minutes and keep it for 60 minutes, and naturally cool it to room temperature to obtain a brown ZnO / g-C3N4 composite photocatalytic material (ZCN-2).
[0041] from Figure 2-5 Characterization shows that the ZnO and g-C3N4 composite material ZCN-2 was successfully obtained. No other impurity peaks appeared in the spectrum, indicating that no other by-products were generated in the composite material. Figure 1 The transmission electron microscopy images show that the ZnO in the ZCN-2 obtained by step-by-step calcination has a cubic porous structure, and g-C3N4 is tightly attached to its surface; Figure 6 and Figure 7 Photoelectric performance characterization shows that ZCN-2 has a good visible light response range and separation and transfer efficiency of photogenerated carriers, corresponding to its excellent photocatalytic performance.
[0042] Example 3
[0043] Step S1: 20 g of urea was placed in a 100 mL covered crucible, and then placed in a muffle furnace. The temperature of the muffle furnace was raised from room temperature to 550 ° C for 36 min and maintained for 4 h. After naturally cooling to room temperature, a yellow block of g-C3N4 was obtained. The block of g-C3N4 was ground to obtain a yellow solid powder. 300 mg of the powder was evenly spread on the bottom of a 100 mL covered crucible and placed in a muffle furnace. The temperature was raised to 500 ° C at a heating rate of 5 ° C / min and maintained for 4 h. After naturally cooling to room temperature, light yellow g-C3N4 nanosheets (CN) were obtained.
[0044] Step S2: 300 mg CN and 3.28 g 2-methylimidazole were mixed and dissolved in 25 mL methanol solution, ultrasonicated for 30 min and then rapidly stirred for 2 h, and then 25 mL methanol zinc acetate solution (the mass of zinc acetate was 1.83 g) was added, and slowly stirred at room temperature for 24 h. The obtained solid methanol was centrifuged 5 times, placed in a drying oven and dried at 60 ° C for 8 h, and then ground to obtain ZIF-8 / g-C3N4;
[0045] Step S3: Put ZIF-8 / g-C3N4 into a covered crucible, place it in a muffle furnace, and in air, heat it from room temperature to 350°C over 66 minutes and keep it for 120 minutes, then heat it to 400°C over 25 minutes and keep it for 60 minutes, and naturally cool it to room temperature to obtain a brown ZnO / g-C3N4 composite photocatalytic material (ZCN-3).
[0046] Example 4
[0047] Step S1: 3.28 g of 2-methylimidazole and 1.83 g of zinc acetate were dissolved in 25 mL of methanol solution to obtain mixed solution A and solution B.
[0048] Step S2: slowly adding solution B to solution A under stirring conditions, stirring rapidly for 2 hours, and then placing under slow stirring conditions for 22 hours, centrifuging with methanol solution and drying for 8 hours to obtain ZIF-8 powder;
[0049] Step S3: Put ZIF-8 into a covered crucible, place it in a muffle furnace, and heat it from room temperature to 350°C in air for 66 minutes and keep it for 120 minutes, then heat it to 400°C for 25 minutes and keep it for 60 minutes, and naturally cool it to room temperature to obtain white ZnO powder. Figure 1 Transmission electron microscopy images and Figure 3 The results of X-ray diffraction patterns show that ZIF-8 is completely decomposed under the calcination conditions to obtain hexagonal wurtzite ZnO, and ZnO forms porous cubes with a size of 200-300nm based on the ZIF-8 skeleton.
[0050] Example 5
[0051] 30 mg of ZCN-2 catalyst was accurately weighed using an electronic balance, dispersed in 100 mL of tetracycline solution (30 mg / L), stirred for 30 min in the dark to allow the catalyst and tetracycline to reach an adsorption-desorption equilibrium state, and then irradiated the above solution using a 300W xenon lamp (λ>400 nm). During the above illumination, 4 mL of solution was extracted at regular intervals, and the catalyst was removed using a 0.45 μm microporous filter membrane to obtain a clear solution. The absorbance of the clear solution was tested using a UV-visible spectrophotometer at λ=358 nm, and the removal rate of tetracycline was finally calculated using the Lambert-Beer law.
[0052] from Figure 8 It can be seen that the tetracycline removal rate of ZCN-2 was 87.57% within 40 min, showing excellent photocatalytic performance. In addition, the degradation rate constant of tetracycline by ZCN-2 was 0.0440 min -1 , and after 5 cycles, the removal rate still remained at 73.33%.
[0053] The above embodiments describe the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments. The above embodiments and descriptions are only for illustrating the principles of the present invention. Without departing from the scope of the principles of the present invention, the present invention may have various changes and improvements, and these changes and improvements all fall within the scope of protection of the present invention.
Claims
1. A method for preparing a 3D / 2D ZnO / g-C3N4 nanocomposite photocatalytic material, characterized in that: The steps include: Step S1: Put urea into a crucible, place it in a muffle furnace for the first calcination to obtain a yellow block g-C3N4, grind the block g-C3N4 in an agate mortar to obtain a solid powder, and calcine the powder g-C3N4 for the second time to obtain g-C3N4 nanosheets; the first calcination temperature is 550°C for 4 hours, and the second calcination temperature is 500°C for 4 hours; Step S2: g-C3N4 nanosheets and 2-methylimidazole are mixed in a methanol solution, ultrasonically dispersed, and then rapidly stirred, and then zinc acetate / methanol solution is added, and stirred at room temperature to obtain ZIF-8 / g-C3N4; Step S3: placing ZIF-8 / g-C3N4 in a muffle furnace, heating the temperature from 20°C to 350°C and keeping the temperature, then heating the temperature to 400°C and keeping the temperature, and cooling the temperature to room temperature to obtain a 3D / 2D ZnO / g-C3N4 nanocomposite photocatalytic material; This step adopts a two-step calcination method, with a heating rate of 5°C / min from 20 to 350°C, a dwell time of 120min at 350°C, a heating rate of 2°C / min from 350 to 400°C, and a dwell time of 60min at 400°C.
2. The method for preparing the 3D / 2D ZnO / g-C3N4 nanocomposite photocatalytic material according to claim 1, characterized in that: In step S2, the ratio of g-C3N4 nanosheets to methanol is 8 mg / mL, and the molar ratio of zinc acetate to 2-methylimidazole is 1:
4.
3. The method for preparing the 3D / 2D ZnO / g-C3N4 nanocomposite photocatalytic material according to claim 1, characterized in that: The calcination gas atmosphere in step S1 and step S3 is air.
4. The method for preparing the 3D / 2D ZnO / g-C3N4 nanocomposite photocatalytic material according to claim 1, characterized in that: The specific steps are: Step S1: 20 g of urea was placed in a 100 mL covered crucible, which was placed in a muffle furnace. The temperature of the muffle furnace was raised from room temperature to 550 ° C for 36 min and maintained for 4 h. After naturally cooling to room temperature, a yellow block of g-C3N4 was obtained. The block of g-C3N4 was ground to obtain a yellow solid powder. 300-500 mg of the powder was evenly spread on the bottom of a 100 mL covered crucible and placed in a muffle furnace. The temperature was raised to 500 ° C at a heating rate of 5 ° C / min and maintained for 4 h. After naturally cooling to room temperature, a light yellow g-C3N4 nanosheet was obtained. Step S2: 200 mg of g-C3N4 nanosheets and 3.28 g of 2-methylimidazole were mixed and dissolved in 25 mL of methanol solution, ultrasonicated for 30 min and then rapidly stirred for 2 h, and then 25 mL of 1.83 g of zinc acetate / methanol solution was added, and slowly stirred at room temperature for 24 h. The obtained solid methanol was centrifuged 5 times, placed in a drying oven at 60 ° C for 8 h, and then ground to obtain ZIF-8 / g-C3N4; Step S3: Put ZIF-8 / g-C3N4 into a covered crucible, place it in a muffle furnace, and heat it from 20°C to 350°C in air for 66 minutes and keep it for 120 minutes, then heat it to 400°C for 25 minutes and keep it for 60 minutes, and naturally cool it to room temperature to obtain a brown-yellow 3D / 2D ZnO / g-C3N4 composite photocatalytic material.
5. Use of the 3D / 2D ZnO / g-C3N4 nanocomposite photocatalytic material prepared by the method according to any one of claims 1 to 4 in the visible light catalytic degradation of tetracycline in water.
Citation Information
Patent Citations
A ZnO photocatalytic material modified with porous carbon and a preparing method thereof
CN107362789A
Method for preparing porous carbon coated magnetic nano molten iron treatment composite material from low-temperature pyrolysis metallic-organic frame
CN108675431A
Semiconductor / g-C3N4 photocatalyst for CO2 reduction and preparation method thereof
CN111054419A
Preparation method and application of CuO nanosheet / g-C3N4 nanosheet heterojunction composite material
CN111659434A
Preparation method of ZIF-8-derived ZnO / g-C3N4 and application of ZIF-8-derived ZnO / g-C3N4 in oxytetracycline sensor
CN114524453A