An integrated treatment method for shield slurry

Through the integrated processing method of shield mud, the waste mud is converted into building materials by using the process of filter press and doping with curing agent, which solves the problems of large land occupation and weak absorption capacity, and achieves resource utilization and cost reduction. The process is simplified and product strength is improved.

CN116253485BActive Publication Date: 2024-10-11TENGDA CONSTR GROUP CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310210924.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-07
Publication Date
2024-10-11
Estimated Expiration
2043-03-07

AI Technical Summary

Technical Problem

In the existing technology, there are problems such as large land resource occupation, weak absorption capacity, long operation cycle and high cost during the shield mud treatment process. In particular, the high moisture content of the mud leads to a large output of waste mud, and the waste in the stockyard or sedimentation tank The demand for land has surged, and the curing process of dewatered slurry is slow, making it difficult to form a certain mechanical strength and prolonging the construction period of the construction site.

Method used

An integrated processing method of shield mud is used to convert waste mud into building materials or landscape parts through the process of filter press - doping with curing agent - direct demoulding after molding - stacking and curing or direct transportation, using pulverized coal A solidifying agent composed of ash, alkali liquid and coal combustion waste residue can realize the secondary utilization of shield mud and reduce the cost of treatment and disposal.

Benefits of technology

It realizes resource utilization of shield mud, reduces treatment and disposal costs, shortens the treatment cycle, improves efficiency, reduces land occupation, avoids secondary pollution caused by long-term accumulation of mud, simplifies the process, and improves product quality. mechanical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004112664870000101
    Figure BDA0004112664870000101
Patent Text Reader

Abstract

The present invention relates to an integrated treatment method for shield mud, the integrated treatment method comprising: filtering the shield mud to obtain a water-reduced material, mixing and stirring the dehydrated material and a curing agent, and then cutting, pressurizing and curing in sequence to obtain a target product; the curing agent is a mixture of fly ash, alkali solution and coal-fired waste residue. The integrated treatment method provided by the present invention realizes the secondary utilization of shield mud by adopting a specific treatment process, so that the obtained product has good mechanical properties, can realize the resource utilization of such solid waste, and reduce the cost of treatment and disposal.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of secondary utilization of resources, and in particular to an integrated processing method for shield mud. Background Art

[0002] At present, modern subway and tunnel excavation often use shield machines for continuous operation, and the shield machine uses mud to construct the mud-water balance system. During the construction process, due to contact with various geological rock and soil layers, a large amount of waste mud is generated. Calculated based on a shield machine with a diameter of 12m, every 1m of construction advancement will generate 113m 3 Waste mud. After the waste mud is screened by the vibrating screen, the part with suitable density is re-injected into the shield machine, and the part without reuse value is left idle. For the disposal of such waste mud, the process of initial sedimentation in the yard and sedimentation tank, and then dehydration and doping with curing agent to prepare building materials is widely used in the treatment and disposal of waste mud.

[0003] For example, CN109293068A discloses a shield mud treatment system, including a shield waste slurry extraction pump, a fully automatic flocculant liquid preparation and addition system, a mud reaction tank, a concentration tank, a clear water tank, and a secondary dewatering screen. The slurry outlet of the shield waste slurry extraction pump and the drug outlet of the fully automatic flocculant liquid preparation and addition system are connected to the mud reaction tank, the output end of the mud reaction tank is connected to the concentration tank, the overflow port of the concentration tank is connected to the clear water tank, the bottom flow outlet of the concentration tank is connected to the secondary dewatering screen through a screw pump, the bottom flow reflux trough of the secondary dewatering screen is connected to the concentration tank, and the slag outlet of the secondary dewatering screen leads to the landfill. It adopts automatic preparation of flocculant solution and mixing with waste slurry, and after concentration treatment, the upper clear liquid is discharged and the bottom flow is dewatered and slag is discharged, which can effectively reduce costs, is less affected by weather, and improves the efficiency of shield waste slurry treatment.

[0004] CN104529109A discloses a method for treating shield mud, which belongs to the field of shield construction. The method includes: using a disc centrifugal system as a treatment system, the disc centrifugal system includes: a disc centrifuge, the feed port of the disc centrifuge is connected to the mud pipeline, and the mud pipeline is provided with a mud pump and a flow valve; the treated shield mud mixture is pumped into the disc centrifuge through the mud pipeline by the mud pump, the feed flow rate of the shield mud mixture is controlled by the flow valve of the mud pipeline, and the working speed of the disc centrifuge is controlled to separate the pumped shield mud mixture into mud and water, the separated water is used as shield recycled water, and the separated solid particles are discharged. The method is simple, easy to implement, and compared with other methods, it occupies a small area in construction, does not need to add flocculants, does not cause secondary pollution to the environment, and is suitable for construction and use in cities.

[0005] But existing technologies have big problems:

[0006] (1) Since the shield mud has an extremely high moisture content (>98%), a large amount of waste mud is produced during the construction process, resulting in a surge in the demand for land for storage yards or sedimentation tanks at the construction site, which increases the construction cost.

[0007] (2) The mud-water separation efficiency in the storage yard or sedimentation tank is very low, and it is difficult to handle the large amount of waste mud generated in a short period of time.

[0008] (3) The dewatered cement slurry solidifies slowly, and it is difficult to form a certain mechanical strength in the early stage. A large area is required for long-term demoulding and subsequent maintenance, which further prolongs the construction period and occupies land resources.

[0009] In summary, conventional abandoned shield mud treatment technology has the problems of large land resource occupation, weak absorption capacity, long operation cycle and high cost. Summary of the invention

[0010] In view of the problems existing in the prior art, the purpose of the present invention is to provide an integrated treatment method for shield mud, which directly converts the waste mud into building materials or landscape pieces through an integrated treatment process of filter pressing - doping with a curing agent - direct demolding after compression molding - stacking maintenance or direct transportation, thereby realizing the resource utilization of the waste mud.

[0011] To achieve this object, the present invention adopts the following technical solutions:

[0012] The present invention provides an integrated treatment method for shield slurry, the integrated treatment method comprising:

[0013] The shield slurry is filtered to obtain a water-reduced material, the dehydrated material and the curing agent are mixed and stirred, and then the material is cut, pressurized and cured to obtain the target product;

[0014] The curing agent is a mixture of fly ash, alkali solution and coal-fired waste residue.

[0015] The integrated treatment method provided by the present invention realizes the secondary utilization of shield mud by adopting a specific treatment process, so that the obtained product has good mechanical properties, can realize the resource utilization of such solid waste, and reduce the treatment and disposal costs.

[0016] In the present invention, the mass ratio of the fly ash, coal combustion waste residue and alkali solution is (18-38):1:(5-10), for example, it can be 18:1:5, 19:1:5, 20:1:5, 21:1:5, 22:1:5, 23:1:5, 24:1:5, 25:1:5, 26:1:5, 27:1:5, 28:1:5, 29:1:5, 30:1:5, 32:1:5, 34:1:5, 36:1:5, 38:1:5, 18:1:6, 18:1:7, 18:1:8, 18:1:9 or 18:1:10, etc., but is not limited to the listed values, and other unlisted values ​​within the range are also applicable.

[0017] In the present invention, the target product may be a building material such as bricks or landscape architecture, etc., which is specifically realized according to the mold in the pressure molding.

[0018] In the present invention, the alkali solution can be a sodium hydroxide solution and / or a potassium hydroxide solution.

[0019] As a preferred technical solution of the present invention, the shield slurry includes drilling ground-connected wall slurry and / or slurry produced by a slurry shield process.

[0020] In the present invention, the shield mud includes quartz, kaolin, calcium feldspar, calcium feldspar, microcline, mica in black jade, magnesium silicate, talc, albite and the like.

[0021] As a preferred technical solution of the present invention, the moisture content of the water-reducing material is 25-35%, for example, it can be 25%, 25.5%, 26%, 26.5%, 27%, 27.5%, 28%, 28.5%, 29%, 29.5%, 30%, 30.5%, 31%, 31.5%, 32%, 32.5%, 33%, 33.5%, 34%, 34.5% or 35%, etc., but is not limited to the listed values, and other values ​​not listed within the range are also applicable.

[0022] As a preferred technical solution of the present invention, the addition amount of the curing agent is 12-16% of the dry matter mass in the shield mud, for example, it can be 12%, 12.2%, 12.4%, 12.6%, 12.8%, 13%, 13.2%, 13.4%, 13.6%, 13.8%, 14%, 14.2%, 14.4%, 14.6%, 14.8%, 15%, 15.2%, 15.4%, 15.6%, 15.8% or 16%, etc., but is not limited to the listed values, and other values ​​not listed within the range are also applicable.

[0023] In the present invention, the preparation process of the curing agent is as follows: the coal-fired waste residue and alkali solution are reacted once to obtain an alkali-slag mixture, and then the mixture is reacted with fly ash for a second time to obtain the curing agent;

[0024] The particle size of the coal-fired waste is 75-5000 μm; the particle size of the fly ash is 5-90 μm; the molar concentration of the alkali solution is 8-12 mol / L, and the fly ash comprises SiO2 55-62%, Al2O3 10-12%, and CaO6-7% by mass percentage; the SiO2 content in the coal-fired waste is 60-63% by mass percentage.

[0025] In the present invention, fly ash and coal waste residue are both materials produced after biomass combustion, and the difference lies in the obvious difference in particle size and content of specific substances. In addition to unburned coal particles, the material also contains a large amount of silicon, iron, aluminum, calcium, magnesium, sodium, potassium, sulfur oxides and various trace elements. The main phase is glass, accounting for 50%-80%; the crystal minerals contained are mullite, α-quartz, calcite, calcium feldspar, calcium silicate, hematite and magnetite, etc., and a small amount of unburned carbon.

[0026] In the present invention, the temperature of the primary reaction is 120-140°C; the time of the primary reaction is 4-5h;

[0027] In the present invention, the sodium oxide in the alkali slag mixture in the secondary reaction is 6-7% of the mass of the fly ash.

[0028] In the present invention, the particle size of coal waste residue and fly ash refers to a particle cluster in any interval within a range, that is, when specifically selected, the interval that can be selected for fly ash is 5-90μm, 5-10μm, 7-15μm, 12-20μm, 18-30μm, 25-37μm, 32-45μm, 42-58μm, 53-64μm, 60-76μm, 72-83μm or 40-90μm, etc. For example, the interval that can be selected for coal waste residue is 75-100μm, 80-500μm, 300-800μm, 1000-2000μm, 2000-5000μm, 1800-3000μm, 90-1000μm or 220-400μm, etc., but it is not limited to the listed values, and other values ​​not listed in the range are also applicable.

[0029] In the present invention, the temperature of the primary reaction is 120-140°C, for example, it can be 120°C, 122°C, 124°C, 126°C, 128°C, 130°C, 132°C, 134°C, 136°C, 138°C or 140°C, but is not limited to the listed values, and other unlisted values ​​within the range are also applicable.

[0030] In the present invention, the time of one reaction is 4-5h, for example, it can be 4h, 4.2h, 4.4h, 4.6h, 4.8h or 5h, but is not limited to the listed values, and other unlisted values ​​within the range are also applicable.

[0031] In the present invention, the alkali in the alkali-slag mixture in the secondary reaction is 6-7% of the mass of the fly ash in terms of sodium oxide, for example, it can be 6%, 6.1%, 6.2%, 6.3%, 6.4%, 6.5%, 6.6%, 6.7%, 6.8%, 6.9% or 7%, etc., but is not limited to the listed values, and other unlisted values ​​within the range are also applicable.

[0032] As a preferred technical solution of the present invention, the stirring speed of the mixed stirring is 30-60r / min, for example, it can be 30r / min, 32r / min, 34r / min, 36r / min, 38r / min, 40r / min, 42r / min, 44r / min, 46r / min, 48r / min, 50r / min, 52r / min, 54r / min, 56r / min, 58r / min or 60r / min, but is not limited to the listed values, and other unlisted values ​​within the range are also applicable.

[0033] As a preferred technical solution of the present invention, the mixing and stirring time is 20-30 min, for example, it can be 20 min, 21 min, 22 min, 23 min, 24 min, 25 min, 26 min, 27 min, 28 min, 29 min or 30 min, but is not limited to the listed values, and other unlisted values ​​within the range are also applicable.

[0034] As a preferred technical solution of the present invention, the pressure of the pressurized molding is 10-80MPa, for example, it can be 10MPa, 12MPa, 14MPa, 16MPa, 18MPa, 20MPa, 22MPa, 24MPa, 26MPa, 28MPa, 30MPa, 32MPa, 34MPa, 36MPa, 38MPa, 40MPa, 42MPa, 44MPa, 46MPa, 48MPa, 50MPa, 52MPa, 54MPa, 56MPa, 58MPa, 60MPa, 62MPa, 64MPa, 66MPa, 68MPa, 70MPa, 72MPa, 74MPa, 76MPa, 78MPa or 80MPa, but is not limited to the listed values, and other values ​​not listed within the range are equally applicable.

[0035] As a preferred technical solution of the present invention, the curing is natural curing.

[0036] As a preferred technical solution of the present invention, the humidity during the curing is 100%.

[0037] As a preferred technical solution of the present invention, the integrated treatment method comprises: filtering the shield slurry to obtain a water-reduced material, mixing and stirring the dehydrated material and a curing agent, and then cutting, pressurizing and curing in sequence to obtain a target product;

[0038] The shield slurry includes drilling ground-connected wall slurry and / or slurry produced by slurry shield process;

[0039] The moisture content of the water-reducing material is 25-35%;

[0040] The amount of the curing agent added is 12-16% of the dry matter mass in the shield mud, and the curing agent is a mixture of fly ash, alkali solution and coal combustion waste residue;

[0041] The stirring speed of the mixing and stirring is 30-60r / min, and the time of the mixing and stirring is 20-30min;

[0042] The pressure of the pressurized molding is 10-80MPa;

[0043] The curing is natural curing, and the humidity during the curing is 100%.

[0044] In the present invention, the processing method can control the corresponding equipment through a preset program set by a PLC controller or a computer, thereby realizing automatic control of the processing process.

[0045] Compared with the prior art solutions, the present invention has the following beneficial effects:

[0046] (1) Compared with sedimentation tank treatment technology, the present invention occupies a small area, has a short treatment cycle, is highly efficient, saves land and thus reduces treatment costs. In addition, it can effectively realize the resource utilization of waste mud and avoid secondary pollution caused by long-term storage of mud.

[0047] (2) Compared with the traditional molding process, the pressure molding in the present invention can realize direct demoulding, accelerate the flowability of the mold, simplify the process, and save time. At the same time, the blocks demoulded by pressure have a certain mechanical strength, can be stacked and maintained, and further reduce the footprint.

[0048] (3) The present invention realizes fully automatic mechanical operation, and has the advantages of simple operation, efficient processing, and suitability for large-scale promotion and application.

[0049] (4) The present invention can effectively solve the problem of large amounts of waste mud treatment and disposal. At the same time, the blocks produced by the present invention can be used as building materials or landscape pieces, thereby realizing the resource utilization of such solid waste and reducing the cost of treatment and disposal. DETAILED DESCRIPTION

[0050] To better illustrate the present invention and facilitate understanding of the technical solution of the present invention, typical but non-limiting embodiments of the present invention are as follows:

[0051] Example 1

[0052] This embodiment provides an integrated shield mud processing method, including:

[0053] The shield slurry is filtered to obtain water-reduced material, the dehydrated material and the curing agent are mixed and stirred, and then the material is cut, pressed and molded, and cured to obtain the target product (brick);

[0054] The shield slurry includes drilling ground-connected wall slurry and / or slurry produced by slurry shield process;

[0055] The moisture content of the water-reducing material is 25%;

[0056] The amount of the curing agent added is 12% of the dry matter mass in the shield mud, and the curing agent is a mixture of fly ash, alkali solution and coal-fired waste residue;

[0057] The stirring speed of the mixing and stirring is 30r / min, and the mixing and stirring time is 30min;

[0058] The pressure of the press molding is 20MPa;

[0059] The curing is natural curing, and the humidity during the curing is 100%.

[0060] The properties of the obtained target product are shown in Table 1.

[0061] Example 2

[0062] This embodiment provides an integrated shield mud processing method, including:

[0063] The shield slurry is filtered to obtain water-reduced material, the dehydrated material and the curing agent are mixed and stirred, and then the material is cut, pressed and molded, and cured to obtain the target product (brick);

[0064] The shield slurry includes drilling ground-connected wall slurry and / or slurry produced by slurry shield process;

[0065] The moisture content of the water-reducing material is 35%;

[0066] The amount of the curing agent added is 12% of the dry matter mass in the shield mud, and the curing agent is a mixture of fly ash, alkali solution and coal-fired waste residue;

[0067] The stirring speed of the mixing and stirring is 30r / min, and the mixing and stirring time is 30min;

[0068] The pressure of the press molding is 20MPa;

[0069] The curing is natural curing, and the humidity during the curing is 100%.

[0070] The properties of the obtained target product are shown in Table 1.

[0071] Example 3

[0072] This embodiment provides an integrated shield mud processing method, including:

[0073] The shield slurry is filtered to obtain water-reduced material, the dehydrated material and the curing agent are mixed and stirred, and then the material is cut, pressed and molded, and cured to obtain the target product (brick);

[0074] The shield slurry includes drilling ground-connected wall slurry and / or slurry produced by slurry shield process;

[0075] The moisture content of the water-reducing material is 30%;

[0076] The amount of the curing agent added is 16% of the dry matter mass in the shield mud, and the curing agent is a mixture of fly ash, alkali solution and coal combustion waste residue;

[0077] The mixing speed is 60r / min, and the mixing time is 30min;

[0078] The pressure of the press molding is 20MPa;

[0079] The curing is natural curing, and the humidity during the curing is 100%.

[0080] The properties of the obtained target product are shown in Table 1.

[0081] Example 4

[0082] This embodiment provides an integrated shield mud processing method, including:

[0083] The shield slurry is filtered to obtain water-reduced material, the dehydrated material and the curing agent are mixed and stirred, and then the material is cut, pressed and molded, and cured to obtain the target product (brick);

[0084] The shield slurry includes drilling ground-connected wall slurry and / or slurry produced by slurry shield process;

[0085] The moisture content of the water-reducing material is 30%;

[0086] The amount of the curing agent added is 12% of the dry matter mass in the shield mud, and the curing agent is a mixture of fly ash, alkali solution and coal-fired waste residue;

[0087] The stirring speed of the mixing and stirring is 30r / min, and the mixing and stirring time is 30min;

[0088] The pressure of the pressurized molding is 80MPa;

[0089] The curing is natural curing, and the humidity during the curing is 100%.

[0090] The properties of the obtained target product are shown in Table 1.

[0091] Example 5

[0092] The difference from Example 1 is only that the alkali solution is replaced by an equal amount of sodium carbonate solution of equal concentration.

[0093] Example 6

[0094] The only difference from Example 1 is that the fly ash is replaced by water glass having the same silicon dioxide content as that in the fly ash.

[0095] Example 7

[0096] The only difference from Example 1 is that the coal-fired waste residue is replaced by water glass having the same silicon dioxide content as that in the coal-fired waste residue.

[0097] Example 8

[0098] The only difference from Example 1 is that the coal-fired waste residue is replaced by an equal amount of fly ash.

[0099] Example 9

[0100] The only difference from Example 1 is that the fly ash is replaced by an equal amount of coal-fired waste slag.

[0101] In the above-mentioned embodiments 1-9, the shield mud used includes quartz, kaolin, calcium feldspar, calcium feldspar, microcline, mica in black jade, magnesium silicate, talc, albite and the like. The preparation process of the curing agent is as follows: coal waste residue and alkali solution are reacted once to obtain an alkali-slag mixture, and then the alkali-slag mixture is reacted with fly ash for a secondary reaction to obtain the curing agent. During the preparation process, the mass ratio of fly ash, coal waste residue and alkali solution is 28.1:1:8.3; the particle size of the coal waste residue is 800-1200μm; the particle size of the fly ash is 20-74μm; the alkali solution is sodium hydroxide with a concentration of 10mol / L; the fly ash includes SiO2 61%, Al2O3 11%, and CaO 7% by mass percentage; the SiO2 in the coal waste residue is 62% by mass percentage; the fly ash and coal waste residue in the above embodiments are respectively obtained by sorting secondary Class C fly ash. The temperature of the primary reaction is 123°C; the time of the primary reaction is 5 hours; the sodium oxide in the alkali slag mixture in the secondary reaction is 6.7% of the mass of the fly ash. During the preparation process, corresponding replacements can be made for the situations in Examples 5-9, that is, the consistency of the entire process is ensured. The obtained solidified product is tested for compressive strength mechanical properties according to ASTM C109 / C109M-2016a, and the obtained data are shown in Table 1.

[0102] Table 1

[0103]

[0104] It can be seen from the results of the above embodiments that the integrated treatment method provided by the present invention directly converts waste mud into building materials or landscape pieces through an integrated treatment process of filter pressing - doping with a curing agent - direct demolding after compression molding - stacking maintenance or direct transportation, thereby realizing the resource utilization of waste mud.

[0105] It is stated that the present invention illustrates the detailed structural features of the present invention through the above embodiments, but the present invention is not limited to the above detailed structural features, that is, it does not mean that the present invention must rely on the above detailed structural features to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the components selected by the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

[0106] The preferred embodiments of the present invention are described in detail above. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical solution of the present invention, and these simple modifications all belong to the protection scope of the present invention.

[0107] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.

[0108] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.

Claims

1. An integrated treatment method for shield mud, characterized in that: The integrated processing method comprises: The shield slurry is filtered to obtain a water-reducing material, the water-reducing material and a curing agent are mixed and stirred, and then the material is cut, pressurized and cured to obtain a target product; The curing agent is a mixture of fly ash, alkali solution and coal waste residue; the mass ratio of the fly ash, coal waste residue and alkali solution is (18-38):1:(5-10); the particle size of the coal waste residue is 75-5000 μm; the particle size of the fly ash is 5-90 μm; The preparation process of the curing agent is as follows: reacting coal waste slag with alkali solution once to obtain an alkali-slag mixture, and then reacting the mixture with fly ash for a secondary reaction to obtain the curing agent; the temperature of the primary reaction is 120-140° C.; the time of the primary reaction is 4-5 hours; the amount of the curing agent added is 12-16% of the dry matter mass in the shield mud.

2. The integrated processing method according to claim 1, characterized in that: The shield slurry includes drilling ground wall slurry and / or slurry produced by slurry shield process.

3. The integrated processing method according to claim 1, characterized in that: The moisture content of the water-reducing material is 25-35%.

4. The integrated processing method according to claim 1, characterized in that: The stirring speed of the mixing and stirring is 30-60 r / min.

5. The integrated processing method according to claim 1, characterized in that: The mixing and stirring time is 20-30 minutes.

6. The integrated processing method according to claim 1, characterized in that: The pressure of the press molding is 10-80 MPa.

7. The integrated processing method according to claim 1, characterized in that: The curing is natural curing.

8. The integrated processing method according to claim 7, characterized in that: The humidity during the curing is 100%.