Maleic anhydride-conjugated diene copolymer microspheres and preparation method and application thereof
By using environmentally friendly solvents and organic initiators in a protective atmosphere to prepare maleic anhydride-conjugated diene copolymer microspheres, the problems of hazardous chemical raw materials and complex processes in the existing technology are solved, and high safety and environmental protection are achieved. Polymer preparation, expanding its application range as a dispersant.
Patent Information
- Application Number
- CN202111522066.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-12-13
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2041-12-13
AI Technical Summary
In the existing technology, the preparation of isoprene-maleic anhydride copolymer requires the use of highly dangerous chemical raw materials and complex processes, and the small molecule dispersant is unstable, which affects the environmental protection and aesthetics of the material. There is no such method. It is used as a dispersant.
Maleic anhydride-conjugated diene copolymer microspheres are prepared in environmentally friendly mixed solvents by free radical polymerization in a protective atmosphere, avoiding the use of hazardous alkyl metal compounds and high boiling point solvents, and using organic peroxides or azo compounds. Acts as an initiator to form stable microsphere polymers and as a dispersant for polypropylene.
The safety and environmental protection of the polymerization reaction are improved. The obtained microsphere polymer has high cleanliness and low odor without washing. As a dispersant, it does not migrate or precipitate in polypropylene, and its stability and application range are expanded.
Smart Images

Figure CN116262802B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of polymers, and in particular to maleic anhydride-conjugated diene copolymer microspheres and a preparation method and application thereof. Background Art
[0002] Conjugated dienes such as isoprene are prone to Diels-Alder reactions with maleic anhydride, which brings certain difficulties to the copolymerization of the two. Maleic anhydride-isoprene copolymers can be obtained through free radical polymerization, reacting in polar solvents such as cyclohexanone and dioxane to obtain polymers containing cis-olefin structural units.
[0003] In the prior art, the preparation of isoprene maleic anhydride polymer requires the use of catalysts with relatively complex structures and chemical raw materials with high flammability and hazard, such as alkyl aluminum, or the use of ester solvents, such as isoamyl acetate. Due to the special interaction between the polymer and the ester solvent, and the special odor of the ester solvent, the material will have an odor even if it contains a small amount of residual ester solvent, and special solvents are required for polymerization and reaction termination, polymer washing and other process processes, and the process safety and environmental protection are poor.
[0004] Traditional dispersants are small organic molecules with a small molecular weight. They are volatile during processing, which is not conducive to environmental protection. Moreover, as the use time increases, the small organic molecule dispersants added to the polymer will migrate to the surface of the polymer, which will affect the appearance and use of the polymer in certain occasions. Currently, there is no isoprene-maleic anhydride copolymer microsphere that can be used as a dispersant in the prior art.
[0005] Therefore, it is urgent to develop a conjugated diene-maleic anhydride copolymer microsphere with dispersion stability that can be used as a polymer dispersant, and the preparation process is reasonable, simple, safe and environmentally friendly, so as to expand the application range of the conjugated diene-maleic anhydride copolymer microsphere. Summary of the invention
[0006] The purpose of the present invention is to overcome the problems of the existing technology that the polymerization of conjugated dienes and maleic anhydride uses dangerous alkyl metal compounds, the process is cumbersome, the product is environmentally friendly, and the existing small molecule dispersant is unstable. A maleic anhydride-conjugated diene copolymer microsphere and its preparation method and application are provided. The maleic anhydride-conjugated diene copolymer microsphere is prepared by a free radical polymerization method in the presence of an environmentally friendly mixed solvent. The polymerization process is highly safe, the process is simple, environmentally friendly, and energy-saving. At the same time, the prepared polymer can be used as a dispersant in polypropylene. Unlike traditional small molecule dispersants, this microsphere polymer does not migrate or precipitate as a dispersant in polypropylene.
[0007] In order to achieve the above-mentioned object, the first aspect of the present invention provides a method for preparing maleic anhydride-conjugated diene copolymer microspheres, characterized in that the method comprises: in a protective atmosphere, dissolving a polymerization monomer and an initiator in a reaction medium to form a homogeneous solution and subjecting the homogeneous solution to a polymerization reaction to obtain a copolymer emulsion suspension, and separating the maleic anhydride-conjugated diene copolymer microspheres;
[0008] Wherein, the polymerizable monomers are maleic anhydride and conjugated diene; based on the total weight of the polymerizable monomers, the amount of maleic anhydride is 35-80wt%, and the amount of conjugated diene is 20-65wt%;
[0009] The reaction medium is a mixture of the compound represented by formula (1) and an alkane;
[0010]
[0011] Among them, R 1 and R 2 Each is independently an alkyl group having 1 to 6 carbon atoms.
[0012] The second aspect of the present invention provides a maleic anhydride-conjugated diene copolymer microsphere, characterized in that the maleic anhydride-conjugated diene copolymer microsphere is prepared by the above method.
[0013] The third aspect of the present invention provides a method for preparing the maleic anhydride-conjugated diene copolymer microspheres and / or the use of the maleic anhydride-isoprene copolymer microspheres as a dispersant in polypropylene.
[0014] Through the above technical scheme, the maleic anhydride-conjugated diene copolymer microspheres provided by the present invention and the preparation method and application thereof obtain the following beneficial effects:
[0015] No alkyl metal compound is required during the reaction, which improves the safety of the reaction;
[0016] No solvents with high boiling points or pungent odors are used during the reaction, making the process environmentally friendly;
[0017] The prepared polymer has high cleanliness and low odor without washing and purification;
[0018] The prepared polymer can be used as a dispersant in polypropylene. Different from traditional small molecule dispersants, the microsphere polymer does not migrate or precipitate as a dispersant in polypropylene. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 This is a scanning electron microscope image of the maleic anhydride-conjugated diene copolymer microspheres of Example 1. DETAILED DESCRIPTION
[0020] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0021] The first aspect of the present invention provides a method for preparing maleic anhydride-conjugated diene copolymer microspheres, characterized in that the method comprises: in a protective atmosphere, dissolving a polymerization monomer and an initiator in a reaction medium to form a homogeneous solution and subjecting the homogeneous solution to polymerization to obtain a copolymer emulsion suspension, and separating the copolymer emulsion suspension to obtain the maleic anhydride-conjugated diene copolymer microspheres;
[0022] Wherein, the polymerizable monomers are maleic anhydride and conjugated diene; based on the total weight of the polymerizable monomers, the amount of maleic anhydride is 35-80wt%, and the amount of conjugated diene is 20-65wt%;
[0023] The reaction medium is a mixture of the compound represented by formula (1) and an alkane;
[0024]
[0025] Among them, R 1 and R 2 Each is independently an alkyl group having 1 to 6 carbon atoms.
[0026] In the present invention, maleic anhydride monomer and conjugated diene are copolymerized in a specific ratio by copolymerization, so that the prepared maleic anhydride-conjugated diene copolymer microspheres have clean surface, uniform particle size, no odor, and stable dispersion in the polymer.
[0027] Furthermore, based on the total weight of the polymerizable monomers, the amount of maleic anhydride is 40-70 wt %, and the amount of the conjugated diene is 30-60 wt %.
[0028] According to the present invention, the conjugated diene is isoprene and / or butadiene.
[0029] According to the present invention, based on the total weight of the homogeneous solution, the total mass concentration of the polymerizable monomers is 2.5-30wt%, preferably 10-18wt%, and the mass concentration of the initiator is 0.05-0.5wt%, preferably 0.08-0.1wt%.
[0030] In the present invention, when the amount of maleic anhydride, the amount of conjugated diene, the mass concentration of the polymerized monomer and the concentration of the initiator all meet the above ranges, the dispersion stability of the prepared maleic anhydride-conjugated diene copolymer microspheres is better.
[0031] According to the present invention, the initiator is an organic peroxide and / or an azo compound.
[0032] According to the present invention, the organic peroxide is at least one selected from dibenzoyl peroxide, diisopropyl peroxide, di-tert-butyl peroxide, dodecyl peroxide, tert-butyl perbenzoate, diisopropyl peroxydicarbonate and dicyclohexyl peroxydicarbonate.
[0033] According to the present invention, the azo compound is selected from azobisisobutyronitrile and / or azobisisoheptanenitrile.
[0034] According to the present invention, in formula (1), R 1 and R 2 Each is independently an alkyl group having 1 to 4 carbon atoms, preferably a methyl group or an ethyl group.
[0035] According to the present invention, the alkane is an alkane having 6 to 12 carbon atoms.
[0036] In the present invention, a mixture of the compound represented by formula (1) and an alkane is selected as the reaction medium, which can avoid the special smell caused by ester solvents, resulting in limited application occasions. The surface of the copolymer microspheres obtained by the present invention is clean, pollution-free and odor-free, thereby increasing the application range in polymers.
[0037] Furthermore, the alkane is selected from at least one of hexane, heptane and octane.
[0038] Furthermore, the alkane is preferably heptane.
[0039] According to the present invention, based on the total volume of the reaction medium, the amount of the alkane is 45-80 vol%, preferably 50-70 vol%.
[0040] According to the present invention, the polymerization reaction is carried out in a protective atmosphere. The protective atmosphere is not particularly limited and can be provided by conventional protective gases in the prior art, such as nitrogen.
[0041] According to the present invention, the conditions of the polymerization reaction include: the polymerization temperature is 61-90° C., preferably 65-85° C.; the polymerization time is 1-20 h, preferably 3-12 h.
[0042] In the present invention, a water bath and / or an oil bath is used to provide the heat required for the polymerization of the present invention.
[0043] In the present invention, the separation may be a conventional solid-liquid separation method in the art, such as centrifugal separation.
[0044] In the present invention, when centrifugal separation is adopted, the centrifugal speed is 1000-5000 rad / min, and the centrifugal time is 5-50 min.
[0045] The second aspect of the present invention provides a maleic anhydride-conjugated diene copolymer microsphere, characterized in that the maleic anhydride-conjugated diene copolymer microsphere is prepared by the above method.
[0046] According to the present invention, the copolymer in the maleic anhydride-conjugated diene copolymer microspheres comprises a structural unit A derived from maleic anhydride and a structural unit B derived from a conjugated diene;
[0047] Based on the total molar amount of each structural unit in the copolymer, the molar content of the structural unit A is 47-53 mol%, and the molar content of the structural unit B is 47-53 mol%.
[0048] Preferably, the molar content of the structural unit A is 47-52 mol%, and the molar content of the structural unit B is 48-52 mol%.
[0049] Furthermore, the molar content of the structural unit A is 48-52 mol%, and the molar content of the structural unit B is 48-51 mol%.
[0050] In the present invention, the molar content of each structural unit in the copolymer of maleic anhydride-conjugated diene copolymer microspheres is tested by elemental analysis.
[0051] According to the present invention, the average particle size of the maleic anhydride-conjugated diene copolymer microspheres is 500-1600 nm, preferably 600-1300 nm.
[0052] In the present invention, the average particle size of the copolymer microspheres is measured by a scanning electron microscope.
[0053] The third aspect of the present invention provides a method for preparing the maleic anhydride-conjugated diene copolymer microspheres and / or the use of the maleic anhydride-isoprene copolymer microspheres as a dispersant in polypropylene.
[0054] In the present invention, the prepared copolymer microspheres are used as dispersants in polypropylene. Unlike traditional small molecule dispersants, the microsphere polymer does not migrate or precipitate in polypropylene. In addition, by using specific solvents and proportions, the copolymer microspheres have no odor and have improved dispersion stability, thereby expanding the scope of application.
[0055] The present invention will be described in detail below by way of examples. In the following examples,
[0056] The polymerization yield (C p ) to calculate
[0057] C p =Mp×100% / Mm
[0058] Wherein, Mp is the mass of the obtained polymer; Mm is the total mass of the added monomers;
[0059] The morphology of copolymer microspheres was observed and measured using scanning electron microscopy (SEM);
[0060] The average particle size of copolymer microspheres was measured by scanning electron microscopy (SEM);
[0061] The tensile strength of polypropylene composites is tested according to GB / T 1040-2006;
[0062] The content of each structural unit in the copolymer was tested by elemental analysis.
[0063] The raw materials used in the examples and comparative examples are all commercially available.
[0064] Example 1
[0065] 9.8g maleic anhydride, 0.1g azobisisobutyronitrile, 8g isoprene, 50ml butanone and 50ml heptane were added to a 2L reactor. After the materials were mixed evenly, the temperature was raised to 70°C and the reaction was carried out for 5 hours. After the reaction was completed, the obtained polymer emulsion suspension was centrifuged at a speed of 2000rad / min for 20 minutes to obtain 12.52g of copolymer microspheres 1M, corresponding to a polymer yield of 70.3%. The size of the copolymer microspheres 1M was 1270nm. The amount of maleic anhydride was 55.1wt%; the amount of isoprene was 44.9wt%; and the amount of heptane in the reaction medium was 50vol%.
[0066] The copolymer microspheres 1M were subjected to elemental analysis, and the results showed that, based on the total molar amount of each structural unit in the polymer, the molar content of the structural unit A derived from maleic anhydride was 49 mol%, and the molar content of the structural unit B derived from isoprene was 51 mol%.
[0067] Example 2
[0068] 2g maleic anhydride, 0.1g azobisisobutyronitrile, 3.4g isoprene, 40ml butanone and 60ml heptane were added to a 2L reactor. After the materials were mixed evenly, the temperature was raised to 90°C and the reaction was carried out for 5h. After the reaction was completed, the obtained polymer emulsion suspension was centrifuged at a speed of 2000rad / min for 20 minutes to obtain 3.2g of copolymer microspheres 2M, corresponding to a polymer yield of 59.3%. The size of the copolymer microspheres 2M was 605nm. The amount of maleic anhydride was 37wt%; the amount of isoprene was 63wt%; and the amount of heptane in the reaction medium was 60vol%.
[0069] The copolymer microspheres 2M were subjected to elemental analysis, and the results showed that based on the total molar amount of each structural unit in the polymer, the molar content of the structural unit A derived from maleic anhydride was 48 mol%, and the molar content of the structural unit B derived from isoprene was 52 mol%.
[0070] Example 3
[0071] 4.9g maleic anhydride, 0.38g azobisisoheptanenitrile, 3.4g isoprene, 20ml acetone and 80ml hexane were added to a 2L reactor. After the materials were mixed evenly, the temperature was raised to 50°C and the reaction was carried out for 5h. After the reaction was completed, the obtained polymer emulsion suspension was centrifuged at a speed of 2000rad / min for 20 minutes to obtain 8g of copolymer microspheres 3M, corresponding to a polymer yield of 96.4%. The size of the copolymer microspheres 3M was 1300nm. The amount of maleic anhydride was 59wt%; the amount of isoprene was 41wt%; and the amount of heptane in the reaction medium was 80vol%.
[0072] The copolymer microspheres 3M were subjected to elemental analysis, and the results showed that based on the total molar amount of each structural unit in the polymer, the molar content of the structural unit A derived from maleic anhydride was 49 mol%, and the molar content of the structural unit B derived from isoprene was 51 mol%.
[0073] Example 4
[0074] 4.9g maleic anhydride, 0.1g azobisisoheptanitrile, 3.4g isoprene, 25ml acetone and 75ml hexane were added to a 2L reactor. After the materials were mixed evenly, the temperature was raised to 50°C and the reaction was carried out for 5h. After the reaction was completed, the obtained polymer emulsion suspension was centrifuged at a speed of 2000rad / min for 20 minutes to obtain 5g of copolymer microspheres 4M, corresponding to a polymer yield of 60.2%. The size of the copolymer microspheres 4M was 900nm. The amount of maleic anhydride was 59wt%; the amount of isoprene was 41wt%; and the amount of heptane in the reaction medium was 75vol%.
[0075] The copolymer microspheres 4M were subjected to elemental analysis, and the results showed that, based on the total molar amount of each structural unit in the polymer, the molar content of the structural unit A derived from maleic anhydride was 50 mol%, and the molar content of the structural unit B derived from isoprene was 50 mol%.
[0076] Example 5
[0077] 4.9g maleic anhydride, 0.1g azobisisoheptanitrile, 6.8g isoprene, 30ml acetone and 70ml hexane were added to a 2L reactor. After the materials were mixed evenly, the temperature was raised to 50°C and the reaction was carried out for 5h. After the reaction was completed, the obtained polymer emulsion suspension was centrifuged at a speed of 2000rad / min for 20 minutes to obtain 8.1g of copolymer microspheres 5M, corresponding to a polymer yield of 69.2%. The size of the copolymer microspheres 5M was 700nm. The amount of maleic anhydride was 41.9wt%; the amount of isoprene was 58.1wt%; and the amount of heptane in the reaction medium was 70vol%.
[0078] The copolymer microspheres 5M were subjected to elemental analysis, and the results showed that based on the total molar amount of each structural unit in the polymer, the molar content of the structural unit A derived from maleic anhydride was 52 mol%, and the molar content of the structural unit B derived from isoprene was 48 mol%.
[0079] Example 6
[0080] 4.9g maleic anhydride, 0.1g azobisisoheptanonitrile, 7g butadiene, 20ml butanone and 80ml heptane were added to a 2L reactor. After the materials were mixed evenly, the temperature was raised to 50°C and the reaction was carried out for 5h. After the reaction was completed, the obtained polymer emulsion suspension was centrifuged at a speed of 2000rad / min for 20 minutes to obtain 7.5g of copolymer microspheres 6M, corresponding to a polymer yield of 63%. The size of the copolymer microspheres 6M was 600nm. The amount of maleic anhydride was 41.2wt%; the amount of isoprene was 58.8wt%; and the amount of heptane in the reaction medium was 80vol%.
[0081] The copolymer microspheres 6M were subjected to elemental analysis, and the results showed that based on the total molar amount of each structural unit in the polymer, the molar content of the structural unit A derived from maleic anhydride was 52 mol%, and the molar content of the structural unit B derived from butadiene was 48 mol%.
[0082] Example 7
[0083] 4.9g maleic anhydride, 0.1g azobisisoheptanenitrile, 7g butadiene, 30ml butanone and 70ml heptane were added to a 2L reactor. After the materials were mixed evenly, the temperature was raised to 50°C and the reaction was carried out for 5h. After the reaction was completed, the obtained polymer emulsion suspension was centrifuged at a speed of 2000rad / min for 20 minutes to obtain 7g of copolymer microspheres 7M, corresponding to a polymer yield of 59%. The size of the copolymer microspheres 7M was 650nm. The amount of maleic anhydride was 41.2wt%; the amount of isoprene was 58.8wt%; and the amount of heptane in the reaction medium was 70vol%.
[0084] The copolymer microspheres 7M were subjected to elemental analysis, and the results showed that based on the total molar amount of each structural unit in the polymer, the molar content of the structural unit A derived from maleic anhydride was 52 mol%, and the molar content of the structural unit B derived from butadiene was 48 mol%.
[0085] Example 8
[0086] Copolymer microspheres were prepared according to the method of Example 1, except that the amount of butanone was 60 mL and the amount of heptane was 40 mL. 8.2 g of copolymer microspheres 8M were obtained, corresponding to a polymer yield of 46.1%. The size of copolymer microspheres 8M was 1300 nm. Among them, the amount of maleic anhydride was 55.1 wt%; the amount of isoprene was 44.9 wt%; and the amount of heptane in the reaction medium was 40 vol%.
[0087] The copolymer microspheres 8M were subjected to elemental analysis, and the results showed that based on the total molar amount of each structural unit in the polymer, the molar content of the structural unit A derived from maleic anhydride was 49 mol%, and the molar content of the structural unit B derived from isoprene was 51 mol%.
[0088] Example 9
[0089] Copolymer microspheres were prepared according to the method of Example 1, except that the amount of maleic anhydride was 11.25 g and the amount of butadiene was 7.5 g. 14 g of copolymer microspheres 9M were obtained, corresponding to a polymer yield of 74.7%. The size of copolymer microspheres 9M was 1300 nm. Among them, the amount of maleic anhydride was 60 wt%; the amount of isoprene was 40 wt%; and the amount of heptane in the reaction medium was 40 vol%.
[0090] The copolymer microspheres 9M were subjected to elemental analysis, and the results showed that, based on the total molar amount of each structural unit in the polymer, the molar content of the structural unit A derived from maleic anhydride was 50 mol%, and the molar content of the structural unit B derived from isoprene was 50 mol%.
[0091] Example 10
[0092] The copolymer microspheres were prepared according to the method of Example 1, except that 20 g of maleic anhydride, 0.2 g of azobisisoheptanitrile, 30 g of isoprene, 50 ml of acetone and 50 ml of heptane were added to a 2 L reactor, the materials were mixed evenly, the temperature was raised to 50°C in a water bath, the reaction was carried out for 5 hours, and a solid substance 10M was obtained after the reaction was completed. The amount of maleic anhydride was 40 wt%; the amount of isoprene was 60 wt%; and the amount of heptane in the reaction medium was 50 vol%.
[0093] Comparative Example 1
[0094] The copolymer microspheres were prepared according to the method of Example 1, except that the reaction medium did not contain alkanes. Specifically, 5 g of maleic anhydride, 0.2 g of azobisisoheptanitrile, 3.5 g of isoprene and 100 ml of acetone were added to a 2 L reactor. After the materials were mixed evenly, the temperature was raised to 50°C and the reaction was carried out for 5 hours. After the reaction was completed, a transparent solution was obtained, and no microspherical polymer material was obtained. The amount of maleic anhydride used was 58.8 wt%; the amount of isoprene used was 41.2 wt%.
[0095] Comparative Example 2
[0096] The copolymer microspheres were prepared according to the method of Example 1, except that the reaction medium did not contain acetone. Specifically, 5 g of maleic anhydride, 0.2 g of azobisisoheptanitrile, 3.5 g of isoprene and 100 ml of heptane were added to a 2L reactor. After the materials were mixed evenly, the temperature was raised to 50°C and the reaction was carried out for 5 hours. After the reaction was completed, a solid mass 2D was obtained instead of a suspension, and no microspherical polymer was obtained. The amount of maleic anhydride was 58.8 wt%; the amount of isoprene was 41.2 wt%; and the amount of heptane in the reaction medium was 100 vol%.
[0097] The solidified copolymer 2D was subjected to elemental analysis, and the molar content of the structural unit A derived from maleic anhydride was 52 mol % and the molar content of the structural unit B derived from isoprene was 48 mol % based on the total molar amount of each structural unit in the polymer.
[0098] Comparative Example 3
[0099] Copolymer microspheres were prepared according to the method of Example 1, except that butanone was replaced by nonanone (R1 is a methyl group, and R2 is an alkyl group with 7 carbon atoms). A solidified copolymer 3D was obtained, wherein the amount of maleic anhydride was 55.1 wt %; the amount of isoprene was 44.9 wt %; and the amount of heptane in the reaction medium was 45 vol %.
[0100] The solidified copolymer 3D was subjected to elemental analysis, and it was found that the molar content of the structural unit A derived from maleic anhydride was 48 mol % and the molar content of the structural unit B derived from isoprene was 52 mol % based on the total molar amount of each structural unit in the polymer.
[0101] Comparative Example 4
[0102] 4.9g maleic anhydride, 0.1g azobisisobutyronitrile, 20g isoprene, 45ml butanone and 55ml heptane were added to a 2L reactor. After the materials were mixed evenly, the temperature was raised to 70°C and the reaction was carried out for 5h. After the reaction was completed, the obtained polymer emulsion suspension was centrifuged at a speed of 2000rad / min for 20 minutes to obtain 6.8g of copolymer microspheres 4D, corresponding to a polymer yield of 58.1%. The size of the copolymer microspheres 4D was 1020mn. The obtained polymer microspheres showed adhesion and aggregation with each other, and the dispersibility was poor. Among them, the amount of maleic anhydride was 19.68wt%; the amount of isoprene was 80.32wt%; and the amount of heptane in the reaction medium was 45vol%.
[0103] The copolymer microspheres 4D were subjected to elemental analysis, and the results showed that based on the total molar amount of each structural unit in the polymer, the molar content of the structural unit A derived from maleic anhydride was 48 mol%, and the molar content of the structural unit B derived from isoprene was 52 mol%.
[0104] Table 1
[0105] Example 1 2 3 4 5 6 7 8 9 10 Maleic anhydride / wt% 55.1 58.8 59 59 419. 41.2 41.2 55.1 60 40 Isoprene / wt% 44.9 41.2 41 41 58.1 58.8 58.8 44.9 40 60 Polymerization monomer concentration / wt% 15.1 5.1 7.7 7.7 10.5 10.6 11.1 15.1 20 33.2 Initiator Type AIBN AIBN ABVN ABVN ABVN ABVN ABVN AIBN AIBN ABVN Initiator concentration / wt% 0.08 0.095 0.5 0.092 0.089 0.089 0.089 0.08 0.08 0.13 Ketone Types Butanone Butanone acetone acetone acetone Butanone Butanone Butanone Butanone acetone Alkane Type Heptane Heptane Hexane Hexane Hexane Heptane Heptane Heptane Heptane Heptane Alkane dosage / vol% 50 60 80 75 70 80 70 40 40 45 Molar content of A / mol% 49 48 49 50 52 52 52 49 50 49 Molar content of B / mol% 51 52 51 50 48 48 48 51 50 51 Copolymer yield / % 70.3 59.3 96.4 60.2 69.2 63 59 46.1 74.7 55 Particle size / nm 1270 605 1300 900 700 600 650 1300 1300 -
[0106] Table 2
[0107]
[0108]
[0109] Test Case
[0110] The maleic anhydride-conjugated diene copolymer microspheres prepared in the examples and comparative examples and conventional dispersants such as ethylene bisstearamide or zinc stearate were respectively used as dispersants to fill polypropylene.
[0111] Maleic anhydride-conjugated diene copolymer microspheres are used as a dispersant in polypropylene and are blended and granulated by a twin-screw extruder, wherein the amount of polypropylene added is 3000g, the amount of 1010 added is 0.25wt% of the polypropylene, the amount of 168 added is 0.25wt% of the polypropylene, the amount of calcium carbonate used is 10wt% of the mass of polypropylene, and the temperatures of each section of the extruder are as follows: 180°C, 200°C, 220°C, 260°C, 260°C, 240°C, 220°C, 200°C.
[0112] The obtained particles were injected to obtain polymer samples for performance testing, and the performance testing was performed again after being placed for half a year. The results are shown in the following table:
[0113] Table 3
[0114]
[0115]
[0116] Note: 0 is the initial tensile strength, t 1 For tensile strength
[0117] It can be seen from the above embodiments and comparative examples that the preparation method provided by the present invention can realize a self-stabilizing precipitation polymerization reaction to obtain a stable polymer microsphere suspension, thereby making the prepared copolymer microspheres have uniform particle size and clean surface without pollution. It can be seen from Table 3 that the tensile strength of the copolymer microsphere polypropylene composite prepared in Examples 1-10 after being stored for half a year is less than 10%, and the performance is relatively stable.
[0118] However, the methods of Comparative Examples 1-4 cannot obtain polymer microspheres with uniform and smooth particle sizes, and therefore cannot be used as dispersants. Even if added to the composite, the obtained polypropylene composite will have poor performance, and its initial tensile strength will not exceed 20 MPa.
[0119] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A method for preparing maleic anhydride-conjugated diene copolymer microspheres, characterized in that: The method comprises: dissolving a polymerization monomer and an initiator in a reaction medium in a protective atmosphere to form a homogeneous solution and subjecting the solution to polymerization reaction to obtain a copolymer emulsion suspension, and separating the suspension to obtain the maleic anhydride-conjugated diene copolymer microspheres; Wherein, the polymerizable monomers are maleic anhydride and conjugated diene; based on the total weight of the polymerizable monomers, the amount of maleic anhydride is 35-80wt%, and the amount of conjugated diene is 20-65wt%; The reaction medium is a mixture of the compound represented by formula (1) and an alkane; Wherein, R1 and R2 are each independently an alkyl group having 1 to 6 carbon atoms; Based on the total weight of the homogeneous solution, the total mass concentration of the polymerization monomer is 2.5-30wt%, and the mass concentration of the initiator is 0.05-0.5wt%; Based on the total volume of the reaction medium, the amount of the alkane used is 45-80 vol%.
2. The preparation method according to claim 1, wherein Based on the total weight of the polymerizable monomers, the amount of maleic anhydride used is 40-70wt%, and the amount of the conjugated diene used is 30-60wt%.
3. The preparation method according to claim 1 or 2, wherein Based on the total weight of the homogeneous solution, the total mass concentration of the polymerizable monomers is 10-18 wt %, and the mass concentration of the initiator is 0.08-0.1 wt %.
4. The preparation method according to claim 1 or 2, wherein: The initiator is selected from organic peroxides and / or azo compounds.
5. The preparation method according to claim 4, wherein: The organic peroxide is at least one selected from dibenzoyl peroxide, diisopropyl peroxide, di-tert-butyl peroxide, dodecyl peroxide, tert-butyl perbenzoate, diisopropyl peroxydicarbonate and dicyclohexyl peroxydicarbonate; And / or, the azo compound is selected from azobisisobutyronitrile and / or azobisisoheptanenitrile.
6. The preparation method according to any one of claims 1 to 2 and 5, wherein: In formula (1), R1 and R2 are each independently an alkyl group having 1 to 4 carbon atoms.
7. The preparation method according to claim 6, wherein: In formula (1), R1 and R2 are each independently a methyl group or an ethyl group.
8. The preparation method according to any one of claims 1-2, 5 and 7, wherein: The alkane is an alkane having 6 to 12 carbon atoms.
9. The preparation method according to claim 8, wherein: The alkane is at least one selected from hexane, heptane and octane.
10. The preparation method according to claim 9, wherein: The alkane is heptane.
11. The preparation method according to any one of claims 1-2, 5, 7, 9-10, wherein: Based on the total volume of the reaction medium, the amount of the alkane used is 50-70 vol%.
12. The preparation method according to any one of claims 1-2, 5, 7, 9-10, wherein: The polymerization reaction conditions include: polymerization temperature of 61-90° C., and polymerization time of 1-20 h.
13. The preparation method according to claim 12, wherein: The polymerization reaction conditions include: polymerization temperature of 65-85° C., and polymerization time of 3-12 h.
14. A maleic anhydride-conjugated diene copolymer microsphere, characterized in that: The maleic anhydride-conjugated diene copolymer microspheres are prepared by the preparation method described in any one of claims 1 to 13.
15. The maleic anhydride-conjugated diene copolymer microspheres according to claim 14, wherein: The copolymer in the maleic anhydride-conjugated diene copolymer microspheres comprises a structural unit A derived from maleic anhydride and a structural unit B derived from a conjugated diene; Based on the total molar amount of each structural unit in the copolymer, the molar content of the structural unit A is 47-53 mol%, and the molar content of the structural unit B is 47-53 mol%.
16. The maleic anhydride-conjugated diene copolymer microspheres according to claim 15, wherein: Based on the total molar amount of each structural unit in the copolymer, the molar content of the structural unit A is 47-52 mol%, and the molar content of the structural unit B is 48-52 mol%.
17. The maleic anhydride-conjugated diene copolymer microspheres according to claim 14 or 15, wherein: The average particle size of the maleic anhydride-conjugated diene copolymer microspheres is 500-1600 nm.
18. The maleic anhydride-conjugated diene copolymer microspheres according to claim 17, wherein: The average particle size of the maleic anhydride-conjugated diene copolymer microspheres is 600-1300 nm.
19. A method for preparing the maleic anhydride-conjugated diene copolymer microspheres according to any one of claims 1 to 13, or use of the maleic anhydride-conjugated diene copolymer microspheres according to any one of claims 14 to 18 as a dispersant in polypropylene.