A kind of high-strength aluminum alloy material with complex phase reinforcement and preparation method thereof
By preparing aluminum alloys with components such as Mg1.25-1.65%, Si4.20-4.65%, and Mg2Si and MgZn2 phases, the poor molding ability of Al-Mg-Si alloy and the corrosion resistance of Al-Zn-Mg-Cu alloy are solved. The problem of insufficient results has achieved high strength, corrosion resistance and good molding capabilities to meet the needs of automobiles and aviation components.
Patent Information
- Application Number
- CN202111514589.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-12-13
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2041-12-13
AI Technical Summary
The existing Al-Mg-Si alloy has poor molding capacity and insufficient strength, and the Al-Zn-Mg-Cu alloy has insufficient corrosion resistance, making it difficult to meet the needs of automobile and aviation components for high strength, corrosion resistance and good molding capabilities.
Mg1.25-1.65%, Si4.20-4.65%, Fe0.07-0.15%, Mn0.25-0.45%, Zn4.30-4.62%, Cr0.15-0.30%, Ti0.61-0.83% were used. B0.01-0.75% and Cu0.09-0.15% aluminum alloys were prepared by melting, casting, heat treatment and hot extrusion processes to form Mg2Si and MgZn2 phases to achieve complex phase enhancement.
The tensile strength and corrosion resistance of aluminum alloys are significantly improved, the fluidity and molding capacity are improved, the preparation process is simplified and the cost is reduced.
Abstract
Description
Technical Field
[0001] The invention relates to a multi-phase reinforced high-strength aluminum alloy material and a preparation method thereof, and the application field of the material is the manufacture of automobile and aviation parts. Background Art
[0002] Al-Mg-Si is a deformed aluminum alloy. The main strengthening phase of the alloy is Mg2Si. It has medium strength (T6 treatment, tensile strength 310MPa), good corrosion resistance and weldability. It is mainly used in the manufacture of automobile hubs and other parts. The typical alloy grade is 6061. In practical applications, it is found that the fluidity of the alloy is poor. When used to prepare automobile hub parts, it is easy to segregate in thick walls. The segregated phase is mainly long strips of AlFeSi, which causes a serious decrease in the mechanical properties of the alloy.
[0003] Al-Zn-Mg-Cu is a heat-treatable aluminum alloy with high strength (T6 treatment, tensile strength 524MPa). Its main strengthening phase is MgZn2. It is mainly used in the manufacture of parts in the aviation field. The typical alloy grade is 7075. It was found during use that the corrosion resistance of the alloy is poor, the preparation process is complex, and the equipment requirements and process conditions are relatively stringent. With the demand for lightweight automobiles, it is required to continue to reduce the weight of automobile parts, thereby reducing CO2 emissions. There is an urgent need for aluminum alloys with good forming ability, high strength, uniform and stable organization; at the same time, the aviation field is also in urgent need of lightweight, high-strength, corrosion-resistant aluminum alloys to replace steel parts in certain parts.
[0004] The main reason for the poor forming ability of Al-Mg-Si alloy is the low Si content of the alloy, and the low strength is due to the difficulty in controlling the size, shape and distribution of the strengthening phase Mg2Si in the alloy; the main reason for the formation of AlFeSi segregation phase is the low content of Mn element that inhibits this phase. The reason for the poor corrosion resistance of Al-Zn-Mg-Cu alloy is the low content of elements such as Cr and Ti in the alloy that increase the self-corrosion potential of the alloy. Summary of the invention
[0005] The purpose of the present invention is to provide a composite phase reinforced aluminum alloy material with good forming ability, high strength and good corrosion resistance and a preparation method thereof for the performance requirements of parts in the automotive field and the aviation field. In order to achieve the above object, the present invention is realized by the following technical scheme, and the composition and mass percentage of the high-strength aluminum alloy are: Mg1.25-1.65%, Si4.20-4.65%, Fe0.07-0.15%, Mn0.25-0.45%, Zn4.30-4.62%, Cr0.15-0.30%, Ti0.61-0.83%, B0.01-0.75%, Cu0.09-0.15%, and the balance is Al.
[0006] The aluminum alloy comprises the following mass percentages: Mg1.25-1.65%, Si4.20-4.65%, Fe0.07-0.15%, Mn0.25-0.45%, Zn4.30-4.62%, Cr0.15-0.30%, Ti0.61-0.83%, B0.01-0.75%, Cu0.09-0.15%, and the balance is Al.
[0007] A method for preparing the aluminum alloy is as follows: 1) Melting the alloy a. Put the aluminum ingot into a crucible furnace for heating and heating. When the temperature rises to 720°C, keep it warm for 10 minutes; b. Add Si, Mn, Cr, Ti, Cu and other alloys in order according to the ratio, heat to 750°C, keep it warm for 15 minutes, and stir; c. Wrap the prepared Zn and Mg alloys with aluminum foil, press them into the bottom of the crucible, let it stand for 1 minute, then put them into the furnace for heating, when the furnace temperature rises to 740°C, keep it warm for 15 minutes, and stir; d. Wrap the prepared Al5Ti1B grain refiner with aluminum foil, press it into the bottom of the crucible, let it stand for 1 minute, stir, then put it into the furnace for heating, when the furnace temperature rises to 740°C, keep it warm for 15 minutes. 2) Casting a. Add slag remover, stir, and remove slag; b. Measure the temperature. When the alloy temperature drops to 690°C, cast the alloy into a graphite mold. 3) Heat treatment a. Use a box-type resistance furnace to perform solution treatment on the alloy at 540℃ / 2h; b. Use a box-type resistance furnace to perform aging treatment on the alloy at 190℃ / 3h. 4) Hot extrusion The alloy is hot extruded at a temperature range of 460-490℃ and a speed of 4m / min, and water-cooled.
[0008] Compared with the prior art, the outstanding advantages of the present invention are:
[0009] The alloy forms Mg2Si and MgZn2 phases at the same time, which has a complex phase strengthening effect, greatly improves the tensile strength of the alloy, and overcomes the disadvantage of insufficient strength of Al-Mg-Si alloy used in automotive parts; the Si content in the alloy is increased to 4.20%-4.65%, while ensuring the strength of the alloy, the fluidity and forming ability of the alloy are improved; the Mn content in the alloy is increased to 0.25-0.45%, which inhibits the production of AlFeSi harmful phases; the Cr content in the alloy is increased to 0.15-0.30%, and the Ti content is increased to 0.61-0.83%, which ensures the corrosion resistance of the alloy and overcomes the disadvantage of insufficient corrosion resistance of Al-Zn-Mg-Cu; the preparation process of the alloy is relatively simple, which reduces the preparation cost of the alloy. DETAILED DESCRIPTION
[0010] According to the present invention, a multi-phase reinforced high-strength aluminum alloy material and a preparation method thereof are provided. The components and mass percentages of the aluminum alloy are: Mg1.25-1.65%, Si4.20-4.65%, Fe0.07-0.15%, Mn0.25-0.45%, Zn4.30-4.62%, Cr0.15-0.30%, Ti0.61-0.83%, B0.01-0.75%, Cu0.09-0.15%, and the balance is Al. The preparation method thereof is: melting alloy, casting, heat treatment, and hot extrusion. Example 1
[0011] Alloy composition (mass percentage): Mg1.35%, Si4.50%, Fe0.07%, Mn0.30%, Zn4.35%, Cr0.20%, Ti0.63%, B0.05%, Cu0.11%, and the balance is Al.
[0012] Alloy preparation: 1) Melting alloy a. Place the aluminum ingot in a crucible furnace for heating. When the temperature rises to 720°C, keep it warm for 10 minutes; b. Add Si, Mn, Cr, Ti, Cu and other alloys in order according to the ratio, heat to 750°C, keep it warm for 15 minutes, and stir; c. Wrap the prepared Zn and Mg alloys with aluminum foil, press them into the bottom of the crucible, let it stand for 1 minute, then put them into the furnace for heating. When the furnace temperature rises to 740°C, keep it warm for 15 minutes and stir; d. Wrap the prepared Al5Ti1B grain refiner with aluminum foil, press it into the bottom of the crucible, let it stand for 1 minute, stir, then put it into the furnace for heating. When the furnace temperature rises to 740°C, keep it warm for 15 minutes. 2) Casting a. Add slag remover, stir, and remove slag; b. Measure the temperature. When the alloy temperature drops to 690°C, cast the alloy into a graphite mold. 3) Heat treatment a. Use a box-type resistance furnace to perform solution treatment on the alloy at 540℃ / 2h; b. Use a box-type resistance furnace to perform aging treatment on the alloy at 190℃ / 3h. 4) Hot extrusion The alloy is hot extruded at a temperature range of 460-490℃ and a speed of 4m / min, and water-cooled.
[0013] After the above preparation and treatment, the alloy has a tensile strength of 436 MPa, a yield strength of 395 MPa, an elongation of 12%, and a self-corrosion potential of -675 mV (SCE) in 3% salt water. Example 2
[0014] Alloy composition (mass percentage): Mg1.40%, Si4.55%, Fe0.07%, Mn0.35%, Zn4.40%, Cr0.25%, Ti0.70%, B0.12%, Cu0.12%, and the balance is Al.
[0015] Alloy preparation: 1) Melting alloy a. Place the aluminum ingot in a crucible furnace for heating. When the temperature rises to 720°C, keep it warm for 10 minutes; b. Add Si, Mn, Cr, Ti, Cu and other alloys in order according to the ratio, heat to 750°C, keep it warm for 15 minutes, and stir; c. Wrap the prepared Zn and Mg alloys with aluminum foil, press them into the bottom of the crucible, let it stand for 1 minute, then put them into the furnace for heating. When the furnace temperature rises to 740°C, keep it warm for 15 minutes and stir; d. Wrap the prepared Al5Ti1B grain refiner with aluminum foil, press it into the bottom of the crucible, let it stand for 1 minute, stir, then put it into the furnace for heating. When the furnace temperature rises to 740°C, keep it warm for 15 minutes. 2) Casting a. Add slag remover, stir, and remove slag; b. Measure the temperature. When the alloy temperature drops to 690°C, cast the alloy into a graphite mold. 3) Heat treatment a. Use a box-type resistance furnace to perform solution treatment on the alloy at 540℃ / 2h; b. Use a box-type resistance furnace to perform aging treatment on the alloy at 190℃ / 3h. 4) Hot extrusion The alloy is hot extruded at a temperature range of 460-490℃ and a speed of 4m / min, and water-cooled.
[0016] After the above preparation and treatment, the alloy has a tensile strength of 445 MPa, a yield strength of 402 MPa, an elongation of 10%, and a self-corrosion potential of -654 mV (SCE) in 3% salt water. Example 3
[0017] Alloy composition (mass percentage): Mg1.60%, Si4.60%, Fe0.10%, Mn0.40%, Zn4.53%, Cr0.29%, Ti0.80%, B0.51%, Cu0.14%, and the balance is Al.
[0018] Alloy preparation: 1) Melting alloy a. Place the aluminum ingot in a crucible furnace for heating. When the temperature rises to 720°C, keep it warm for 10 minutes; b. Add Si, Mn, Cr, Ti, Cu and other alloys in order according to the ratio, heat to 750°C, keep it warm for 15 minutes, and stir; c. Wrap the prepared Zn and Mg alloys with aluminum foil, press them into the bottom of the crucible, let it stand for 1 minute, then put them into the furnace for heating. When the furnace temperature rises to 740°C, keep it warm for 15 minutes and stir; d. Wrap the prepared Al5Ti1B grain refiner with aluminum foil, press it into the bottom of the crucible, let it stand for 1 minute, stir, then put it into the furnace for heating. When the furnace temperature rises to 740°C, keep it warm for 15 minutes. 2) Casting a. Add slag remover, stir, and remove slag; b. Measure the temperature. When the alloy temperature drops to 690°C, cast the alloy into a graphite mold. 3) Heat treatment a. Use a box-type resistance furnace to perform solution treatment on the alloy at 540℃ / 2h; b. Use a box-type resistance furnace to perform aging treatment on the alloy at 190℃ / 3h. 4) Hot extrusion The alloy is hot extruded at a temperature range of 460-490℃ and a speed of 4m / min, and water-cooled.
[0019] After the above preparation and treatment, the alloy has a tensile strength of 452 MPa, a yield strength of 415 MPa, an elongation of 6%, and a self-corrosion potential of -646 mV (SCE) in 3% salt water.
Claims
1. A multi-phase reinforced high-strength aluminum alloy material, characterized in that: The components of the aluminum alloy and their mass percentages are: Mg 1.25-1.35%, Si 4.20-4.65%, Fe 0.07-0.15%, Mn 0.25-0.45%, Zn 4.30-4.62%, Cr 0.20-0.30%, Ti 0.61-0.83%, B 0.01-0.75%, Cu 0.09-0.15%, and the balance is Al.
2. The method for preparing a multi-phase reinforced high-strength aluminum alloy material according to claim 1, characterized in that: 1) Melting alloy a. Place the aluminum ingot into a crucible furnace for heating. When the temperature reaches 720°C, keep it warm for 10 minutes. b. Add Si, Mn, Cr, Ti, and Cu alloys in order according to the ratio, raise the temperature to 750°C, keep warm for 15 minutes, and stir; c. Wrap the prepared Zn and Mg alloys with aluminum foil, press them into the bottom of the crucible, let them stand for 1 minute, then heat them in a furnace. When the furnace temperature rises to 740°C, keep them warm for 15 minutes and stir; d. Wrap the prepared Al5Ti1B grain refiner with aluminum foil, press it into the bottom of the crucible, let it stand for 1 minute, stir it, and then heat it in a furnace. When the furnace temperature rises to 740°C, keep it warm for 15 minutes; 2) Casting a. Add slag remover, stir and remove slag; b. Temperature measurement. When the alloy temperature drops to 690°C, the alloy is cast into a graphite mold; 3) Heat treatment a. Use a box-type resistance furnace to perform solution treatment on the alloy at 540℃ / 2h; b. Use a box-type resistance furnace to perform aging treatment on the alloy at 190℃ / 3h; 4) Hot extrusion The alloy was hot extruded at a temperature range of 460-490 °C at a speed of 4 m / min and water-cooled.