Preparation method and application of heat storage and temperature regulating composite phase change nonwoven fabric

The graphene oxide/boron nitride composite phase change non-woven fabric prepared through wet spinning and vacuum impregnation processes solves the leakage and flow problems of phase change materials during heat treatment, achieves high load capacity and high thermal stability, and is suitable for For thermal management of human clothing.

CN116263030BActive Publication Date: 2024-10-01DALIAN INSTITUTE OF CHEMICAL PHYSICS CHINESE ACADEMY OF SCIENCES
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111532077.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-15
Publication Date
2024-10-01
Estimated Expiration
2041-12-15

AI Technical Summary

Technical Problem

Existing phase change materials are prone to leakage and flow during heat treatment, and it is difficult to achieve high coverage rates and high phase change enthalpy values, which limits their promotion in practical applications.

Method used

Using wet spinning and vacuum impregnation processes, hybrid fibers are prepared by mixing ultrasonic treatment of the spinning solution of graphene oxide and boron nitride, and then assembled into non-woven fabrics through suction filtration and autowetting dissolution, and finally under vacuum conditions Mixed with phase change materials to prepare composite phase change non-woven fabrics with high loading capacity and high thermal stability.

Benefits of technology

A leak-free, long-life phase change material has been realized, which can maintain the temperature in the temperature range of 20-38°C for 2-6 hours. It is suitable for thermal management of human clothing and has high load capacity and good thermal stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0003411731470000011
    Figure HDA0003411731470000011
  • Figure HDA0003411731470000012
    Figure HDA0003411731470000012
  • Figure HDA0003411731470000013
    Figure HDA0003411731470000013
Patent Text Reader

Abstract

The invention discloses a preparation method and application of a heat storage and temperature regulating composite phase change non-woven fabric. A suspension of graphene oxide and water is mixed with boron nitride I, and a uniform spinning solution is obtained by stirring and ultrasonication; an ionic liquid salt coagulation bath solution is prepared; the obtained spinning solution is placed in a spinning propulsion device; the terminal outlet is placed in the obtained coagulation bath to obtain hybrid fibers; the obtained hybrid fibers are crushed and filtered, and the filtered self-assembled into non-woven fabrics; the obtained non-woven fabric is placed in a reducing solution and heated to 30-80°C for reduction, and then freeze-dried to obtain the reduced non-woven fabric. The obtained non-woven fabric and phase change material are mixed together, and vacuum impregnated at 50-80°C to obtain a phase change non-woven fabric. Different phase change materials can be added to obtain phase change non-woven fabrics with different phase change temperatures. At the same time, good effects are shown in the application of human body fabric temperature control.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of thermochemical technology, and in particular to a preparation method of a phase-change nonwoven fabric of a human body intelligent temperature-controlling fabric and application thereof. Background Art

[0002] Phase change materials with heat storage and temperature regulation functions are increasingly understood and recognized by people, and their application scope is also becoming increasingly wide. However, due to the leakage, fluidity and environmental compatibility of liquid substances, most materials with phase change heat storage and temperature regulation functions cannot be used directly, so the modification method of phase change materials is still the key technology to promote their practical application. In order to solve the above problems, different solutions are adopted for different materials.

[0003] For higher fatty acids, higher fatty alcohols and organic polymer materials with active functional groups, chemical modification methods are used to synthesize new products to become new solid-solid phase change materials (Haixia Wang, Haifeng Shi, Miao Qi, Lingjian Zhang, Xingxiang Zhang, Lu Qi. Structure and thermal performance of poly (styrene-co-maleic anhydride)-g-alkyl alcohol comb-like copolymeric phase change materials, Thermochimica Acta, 564 (2013) 34–38; Luntao Liu, Haixia Wang, Xiaokang Qi, Lei Kong, Jianping Cui, Xingxiang Zhang, Haifeng Shi. Shape-stabilized phase change materials based on poly (ethylene-graftmaleic anhydride)-g-alkyl alcohol comb-like polymers, Solar Energy Materials & Solar Cells 143 (2015) 21–28.). For long-chain alkane paraffin, microencapsulation is often used to encapsulate the paraffin to form micron-sized particles with a core-shell structure, so as to prevent leakage and flow of the paraffin when heated, and to apparently become a solid-solid phase change material. The chemical reaction process mainly involved in the above methods generally has many steps, a complex reaction system, and even by-products, which makes it difficult to meet the requirements of green production. There are also other polymer materials that are difficult to melt as support carriers, and such phase change functional materials are mixed with them to form a two-component or multi-component organic composite phase change material, which relies on intermolecular forces to hinder the overflow of the phase change functional material melted by heat, thereby forming a fixed-shape phase change material with a certain stability. However, the mechanical strength of this fixed-shape phase change material is low, and long-term use will inevitably lead to slow leakage of liquid materials.

[0004] By using the impregnation method, inorganic materials with natural pores such as expanded perlite, diatomite, and graphite are used as support carriers and mixed with organic phase change functional materials to obtain organic / inorganic composite phase change materials (Lingjian Zhang, Haifeng Shi, Weiwei Li, Xu Han, Xingxiang Zhang. Structure and thermal performance of poly(ethylene glycol)alkyl ether(Brij) / porous silica(MCM-41)composites as shape-stabilized phase change materials, Thermochimica Acta 570(2013)1–7.). However, whether vacuum impregnation, solution impregnation, or melt impregnation is used, it is difficult to obtain a shape-stabilized phase change material with a high coverage rate, because the above methods cannot completely remove the gas therein, and there are still gaps in the obtained material, resulting in a low content of phase change functional materials and a low phase change enthalpy value.

[0005] Using alkanes as phase change functional materials and carbon-based non-woven fabrics as carrier materials, composite non-woven fabric phase change materials can be prepared by wet spinning and vacuum impregnation. The spinning solution is first prepared with graphene oxide suspension and boron nitride as raw materials, and wet spinning is carried out in an ethanol coagulation bath, and non-woven fabrics are obtained by filtration. Then, the non-woven fabrics are fully mixed with alkanes with different phase change temperatures under vacuum to form non-woven composite phase change materials. This product has no voids, high alkane content, high phase change enthalpy, and long thermal cycle life. Summary of the invention

[0006] The present invention discloses a preparation method of an alkane phase change material / graphene fiber composite phase change nonwoven fabric by wet spinning, vacuum impregnation, etc. The prepared graphene oxide suspension and boron nitride are used as raw materials, and a uniform spinning solution of graphene oxide / boron nitride is prepared by mixed ultrasonic treatment; hybrid fibers are prepared by wet spinning, and phase change nonwoven fabrics are prepared by suction filtration and self-wet dissolution assembly, and finally the phase change nonwoven fabrics are prepared by reducing and vacuum impregnating the phase change material.

[0007] The preparation method of the composite phase-change nonwoven fabric comprises the following steps: wet spinning a spinning solution containing graphene oxide and boron nitride to obtain hybrid fibers, wherein the hybrid fibers are self-assembled into a nonwoven fabric, and the nonwoven fabric is reduced; and then vacuum impregnation is performed on a mixture of the reduced nonwoven fabric and a phase-change material to obtain the composite phase-change nonwoven fabric.

[0008] Optionally, the preparation method of the composite phase change nonwoven fabric comprises the following process steps:

[0009] (1) mixing a suspension of graphene oxide and water with boron nitride, and obtaining a uniform spinning solution through stirring and ultrasonication;

[0010] (2) preparing an ionic liquid salt coagulation bath solution;

[0011] (3) placing the spinning solution obtained in (1) in a spinning propulsion device; placing the terminal outlet of the spinning propulsion device in the coagulation bath obtained in (2) to obtain hybrid fibers; crushing the obtained hybrid fibers and filtering them by suction, and filtering and self-assembling them into non-woven fabrics;

[0012] (4) The nonwoven fabric obtained in (3) is placed in a reducing solution and heated to 30 to 80° C. for reduction, and then freeze-dried to obtain the reduced nonwoven fabric.

[0013] (5) The nonwoven fabric obtained in (4) and the phase change material are mixed together and vacuum impregnated at 50 to 80° C. to obtain a phase change nonwoven fabric.

[0014] Optionally, the mixing I is carried out by stirring for more than 30 minutes and then ultrasonically treating for more than 1 hour.

[0015] Optionally, the concentration of graphene oxide in the suspension is 8-30 mg / ml.

[0016] Optionally, the mass ratio of graphene oxide to boron nitride is GO / BN=4-1.

[0017] Optionally, the coagulation bath solution contains a solvent, and the solvent is ethanol.

[0018] Optionally, the concentration of the ionic liquid salt in the coagulation bath solution is 1-2 g / 100 ml ethanol.

[0019] Optionally, the ionic liquid salt is 1-ethyl-3-methylimidazolium chloride or 1-ethyl-3-methylimidazolium bromide.

[0020] Optionally, when the spinning is advanced, the ambient temperature is between 5 and 70° C.; and the diameter of the syringe selected for the spinning is 0.4 to 0.9 mm.

[0021] Optionally, the reducing solution is an aqueous solution of stannous chloride with a mass fraction greater than 1.5%, or an aqueous solution of ascorbic acid with a mass fraction greater than 2%, or a hydroiodic acid solution with a mass fraction greater than 10%.

[0022] Optionally, the ambient temperature when reducing the nonwoven fabric is in the range of 30 to 80° C., and the reduction time is 2 to 24 hours;

[0023] Optionally, the freeze-drying conditions are a temperature of -60°C to -40°C and a pressure of 10Pa to 90Pa.

[0024] Optionally, the phase change material is an alkane phase change material, selected from any one of octadecane, eicosane, and paraffin.

[0025] Optionally, the vacuum impregnation time needs to be 2 hours to 24 hours.

[0026] The present invention also provides a composite phase-change nonwoven fabric obtained by any of the above-mentioned preparation methods.

[0027] The present invention also provides an application of the composite phase-change nonwoven fabric, wherein the composite phase-change nonwoven fabric is used as a heat storage and temperature-regulating phase-change material, and maintains the temperature for 2 to 6 hours in a temperature range of 20-38°C.

[0028] The process conditions of the present invention are low, and the prepared phase change material / hybrid fiber composite phase change material non-woven fabric is in sheet form, has the characteristics of no leakage and long cycle life, and can be adjusted in thickness, and can be used for thermal management of human clothing.

[0029] In the composite phase change material prepared by the method, a three-dimensional network is formed in the hybrid fiber, which has an extremely high loading capacity for the phase change material and high thermal stability, and can be used for heat storage and temperature regulation in human clothing and the like.

[0030] The present invention constructs a preparation method of an alkane phase change material / graphene fiber composite phase change nonwoven fabric by wet spinning, vacuum impregnation, etc. The prepared graphene oxide suspension and amino-modified boron nitride are used as raw materials, and a uniform spinning solution of graphene oxide / boron nitride is prepared by mixed ultrasonic treatment; hybrid fibers are prepared by wet spinning, and phase change nonwoven fabrics are prepared by suction filtration and self-wet dissolution assembly, and finally, phase change nonwoven fabrics are prepared by vacuum impregnation of phase change materials. During the vacuum impregnation process, different phase change materials can be added to obtain phase change nonwoven fabrics with different phase change temperatures. At the same time, good effects are shown in the application of human body fabric temperature control. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 A physical picture of the phase change nonwoven fabric prepared in Example 1 of the present invention.

[0032] Figure 2 A scanning electron microscope image of a single fiber in the phase change nonwoven fabric prepared in Example 1 of the present invention.

[0033] Figure 3 The thermal gravimetric curve of eicosane and the thermal gravimetric curve of the eicosane-composite hybrid fiber phase change nonwoven fabric prepared in Example 1 of the present invention.

[0034] Figure 4 The differential scanning calorimetry curve of eicosane and the differential scanning calorimetry curve of the eicosane-composite hybrid fiber phase change nonwoven fabric prepared in Example 1 of the present invention.

[0035] Figure 5Physical adsorption isotherm of the dried boron nitride hybridized graphene non-woven fabric prepared in (6) of Example 1 of the present invention. DETAILED DESCRIPTION

[0036] The present application is described in detail below with reference to embodiments, but the present application is not limited to these embodiments.

[0037] Unless otherwise specified, the raw materials in the examples of this application were purchased from commercial sources. If the specific conditions are not specified in the examples, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments is not specified, they are all conventional products that can be purchased commercially.

[0038] The morphological characteristics of the samples were tested and analyzed by scanning electron microscopy (SEM), the analysis instrument was JSM7900F, the pore analysis was performed by a physical adsorption instrument, model ASAP 2020, and the thermal gravimetric curve of the samples was tested by a thermogravimetric instrument.

[0039] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.

[0040] Example 1

[0041] (1) 10 ml of a suspension of 8 mg / ml of graphene oxide concentrate was prepared, 20 mg of amino-modified boron nitride powder was added, stirred for 1 h, and ultrasonicated for 2 h to obtain a spinning solution.

[0042] (2) Dissolve 1.5 g of 1-ethyl-3-methylimidazolium chloride in 100 ml of anhydrous ethanol to prepare a coagulation bath.

[0043] (3) The spinning solution obtained in (1) is placed in a spinning apparatus, injected into the coagulation bath of (2), maintained at room temperature of 20° C., and spun to obtain boron nitride hybridized graphene oxide fibers.

[0044] (4) The boron nitride hybridized graphene oxide fibers obtained in (3) are mixed with an appropriate amount of water to obtain a suspension, wherein the amount of water used is based on immersing the fibers. The fibers are cut into short fibers of 1-2 cm in water, and the suspension is filtered. During the filtration process, a layered boron nitride hybridized graphene oxide non-woven fabric can be obtained on the surface of the filter paper through a wet dissolution assembly method.

[0045] (5) The nonwoven fabric obtained in (4) is placed in 1.5 g of stannous chloride / 100 ml of deionized water, heated to 50° C., and kept warm for 12 h. In this process, the boron nitride hybridized graphene oxide nonwoven fabric is reduced to a boron nitride hybridized graphene nonwoven fabric.

[0046] (6) The non-woven boron nitride hybridized graphene non-woven fabric obtained in (5) is freeze-dried (-40°C, 70 Pa) to obtain a dry boron nitride hybridized graphene non-woven fabric.

[0047] (7) The boron nitride hybridized graphene nonwoven fabric obtained in (6) is immersed in liquid eicosane at 60° C., and allowed to stand under vacuum conditions, and maintained at 60° C. for about 24 hours to obtain a black sheet of eicosane-compounded hybrid fiber phase change nonwoven fabric, such as Figure 1 shown.

[0048] Among them, the diameter of a single fiber in the eicosane-compounded hybrid fiber phase change nonwoven fabric is about 320 μm.

[0049] The thermal weight loss curve of the hybrid fiber phase change nonwoven fabric composited with eicosane is as follows Figure 3 As shown, for comparison, Figure 3 The thermal weight loss curve of pure eicosane is also given in Figure 1. It can be seen that the thermal decomposition of eicosane / hybrid fiber composite phase change material shows obvious thermal hysteresis compared with pure eicosane, indicating that the thermal stability of the composite phase change material is better than that of pure eicosane.

[0050] from Figure 4 It can be seen that the mass percentage of eicosane in the eicosane-compounded hybrid fiber phase change nonwoven fabric is about 86%, and the phase change enthalpy is 202 J / g.

[0051] from Figure 5 It can be seen that the eicosane-composite hybrid fiber nonwoven fabric contains a large number of mesopores and has a specific surface area of ​​340 m 2 / g, which is conducive to the entry of phase change materials and prevents solid-liquid leakage during the phase change process.

[0052] Example 2

[0053] (1) 10 ml of a 20 mg / ml suspension of graphene oxide concentrate was prepared, 200 mg of amino-modified boron nitride powder was added, stirred for 0.5 h, and ultrasonicated for 4 h to obtain a spinning solution.

[0054] (2) Dissolve 1 g of 1-ethyl-3-methylimidazolium bromide in 100 ml of anhydrous ethanol to prepare a coagulation bath.

[0055] (3) The spinning solution obtained in (1) is placed in a spinning apparatus, injected into the coagulation bath of (2), maintained at room temperature of 35° C., and spun to obtain boron nitride hybridized graphene oxide fibers.

[0056] (4) The boron nitride hybridized graphene oxide fibers obtained in (3) are mixed with an appropriate amount of water to obtain a suspension, wherein the amount of water used is based on immersing the fibers. The fibers are cut into short fibers of 1-2 cm in water, and the suspension is filtered. During the filtration process, a layered boron nitride hybridized graphene oxide non-woven fabric can be obtained on the surface of the filter paper through a wet dissolution assembly method.

[0057] (5) The nonwoven fabric obtained in (4) is placed in 2 g ascorbic acid / 100 ml deionized water, heated to 70° C., and kept warm for 24 h. In this process, the boron nitride hybridized graphene oxide nonwoven fabric is reduced to a boron nitride hybridized graphene nonwoven fabric.

[0058] (6) The non-woven boron nitride hybridized graphene non-woven fabric obtained in (5) is freeze-dried (-50°C, 90Pa) to obtain a dry boron nitride hybridized graphene non-woven fabric.

[0059] (7) The boron nitride hybridized graphene nonwoven fabric obtained in (6) was immersed in liquid octadecane at 50° C., allowed to stand under vacuum conditions, and maintained at 50° C. for about 2 hours to obtain a black sheet-like eicosane-compounded hybrid fiber phase change nonwoven fabric.

[0060] Example 3

[0061] (1) 10 ml of a 15 mg / ml suspension of graphene oxide concentrate was prepared, 75 mg of amino-modified boron nitride powder was added, stirred for 1.5 h, and ultrasonicated for 1 h to obtain a spinning solution.

[0062] (2) Dissolve 2 g of 1-ethyl-3-methylimidazolium chloride in 100 ml of anhydrous ethanol to prepare a coagulation bath.

[0063] (3) The spinning solution obtained in (1) is placed in a spinning apparatus, injected into the coagulation bath of (2), maintained at room temperature of 20° C., and spun to obtain boron nitride hybridized graphene oxide fibers.

[0064] (4) The boron nitride hybridized graphene oxide fibers obtained in (3) are mixed with an appropriate amount of water to obtain a suspension, wherein the amount of water used is based on immersing the fibers. The fibers are cut into short fibers of 1-2 cm in water, and the suspension is filtered. During the filtration process, a layered boron nitride hybridized graphene oxide non-woven fabric can be obtained on the surface of the filter paper through a wet dissolution assembly method.

[0065] (5) The nonwoven fabric obtained in (4) is placed in a 10% by mass hydroiodic acid solution and maintained at 30° C. for 2 hours. In this process, the boron nitride hybridized graphene oxide nonwoven fabric is reduced to a boron nitride hybridized graphene nonwoven fabric.

[0066] (6) The non-woven boron nitride hybridized graphene non-woven fabric obtained in (5) is freeze-dried (-60°C, 30 Pa) to obtain a dry boron nitride hybridized graphene non-woven fabric.

[0067] (7) The boron nitride hybridized graphene nonwoven fabric obtained in (6) was immersed in liquid eicosane at 60° C., allowed to stand under vacuum conditions, and maintained at 70° C. for about 12 hours to obtain a black sheet-like eicosane-compounded hybrid fiber phase change nonwoven fabric.

[0068] Example 4

[0069] (1) 10 ml of a 30 mg / ml suspension of graphene oxide concentrate was prepared, 150 mg of amino-modified boron nitride powder was added, stirred for 1 h, and ultrasonicated for 2 h to obtain a spinning solution.

[0070] (2) Dissolve 2 g of 1-ethyl-3-methylimidazolium bromide in 100 ml of anhydrous ethanol to prepare a coagulation bath.

[0071] (3) The spinning solution obtained in (1) is placed in a spinning apparatus, injected into the coagulation bath of (2), maintained at room temperature of 20° C., and spun to obtain boron nitride hybridized graphene oxide fibers.

[0072] (4) The boron nitride hybridized graphene oxide fibers obtained in (3) are mixed with an appropriate amount of water to obtain a suspension, wherein the amount of water used is based on immersing the fibers. The fibers are cut into short fibers of 1-2 cm in water, and the suspension is filtered. During the filtration process, a layered boron nitride hybridized graphene oxide non-woven fabric can be obtained on the surface of the filter paper through a wet dissolution assembly method.

[0073] (5) The nonwoven fabric obtained in (4) is placed in 3 g of stannous chloride / 100 ml of deionized water, heated to 80° C., and kept warm for 9 h. In this process, the boron nitride hybridized graphene oxide nonwoven fabric is reduced to a boron nitride hybridized graphene nonwoven fabric.

[0074] (6) The non-woven boron nitride hybridized graphene non-woven fabric obtained in (5) is freeze-dried (-60°C, 10Pa) to obtain a dry boron nitride hybridized graphene non-woven fabric.

[0075] (7) The boron nitride hybridized graphene nonwoven fabric obtained in (6) is immersed in liquid paraffin at 80° C., allowed to stand under vacuum conditions, and maintained at 80° C. for about 16 hours to obtain a black flaky paraffin-compounded hybrid fiber phase change nonwoven fabric.

[0076] Example 5

[0077] (1) 10 ml of a 25 mg / ml suspension of graphene oxide concentrate was prepared, 100 mg of amino-modified boron nitride powder was added, stirred for 3 h, and ultrasonicated for 6 h to obtain a spinning solution.

[0078] (2) Dissolve 1 g of 1-ethyl-3-methylimidazolium chloride in 100 ml of anhydrous ethanol to prepare a coagulation bath.

[0079] (3) The spinning solution obtained in (1) is placed in a spinning apparatus, injected into the coagulation bath of (2), maintained at room temperature of 25° C., and spun to obtain boron nitride hybridized graphene oxide fibers.

[0080] (4) The boron nitride hybridized graphene oxide fibers obtained in (3) are mixed with an appropriate amount of water to obtain a suspension, wherein the amount of water used is based on immersing the fibers. The fibers are cut into short fibers of 1-2 cm in water, and the suspension is filtered. During the filtration process, a layered boron nitride hybridized graphene oxide non-woven fabric can be obtained on the surface of the filter paper through a wet dissolution assembly method.

[0081] (5) The nonwoven fabric obtained in (4) is placed in 3 g ascorbic acid / 100 ml deionized water, heated to 60° C., and kept warm for 18 h. In this process, the boron nitride hybridized graphene oxide nonwoven fabric is reduced to a boron nitride hybridized graphene nonwoven fabric.

[0082] (6) The non-woven boron nitride hybridized graphene non-woven fabric obtained in (5) is freeze-dried (-45°C, 40 Pa) to obtain a dry boron nitride hybridized graphene non-woven fabric.

[0083] (7) The boron nitride hybridized graphene nonwoven fabric obtained in (6) is immersed in liquid polyethylene glycol at 80° C., allowed to stand under vacuum conditions, and maintained at 80° C. for about 4 hours to obtain a black sheet-like polyethylene glycol-compounded hybrid fiber phase change nonwoven fabric.

Claims

1. A method for preparing a composite phase change nonwoven fabric, characterized in that: Wet spinning a spinning solution containing graphene oxide and amino-modified boron nitride to obtain hybrid fibers, wherein the hybrid fibers are self-assembled into a non-woven fabric, and the non-woven fabric is reduced; and then vacuum impregnation of a mixture of the reduced non-woven fabric and the phase change material is performed to obtain the composite phase change non-woven fabric; The method comprises the steps of: (1) mixing a suspension of graphene oxide and water with amino-modified boron nitride, and obtaining a uniform spinning solution through stirring and ultrasonication; (2) preparing an ionic liquid salt coagulation bath solution; (3) placing the spinning solution obtained in (1) in a spinning propulsion device; The terminal outlet is placed in the coagulation bath obtained in (2) to obtain hybrid fibers; the obtained hybrid fibers are crushed and filtered, and the fibers are self-assembled into non-woven fabrics by filtering; (4) placing the nonwoven fabric obtained in (3) in a reducing solution and heating it to 30-80° C. for reduction, and then freeze-drying to obtain the reduced nonwoven fabric; (5) mixing the nonwoven fabric obtained in (4) and the phase change material, and vacuum impregnating the mixture at 50-80° C. to obtain a phase change nonwoven fabric; The mass ratio of the graphene oxide to the amino-treated boron nitride is GO / BN=4-1; The phase change material is an alkane phase change material, selected from any one of octadecane, eicosane and paraffin.

2. The preparation method according to claim 1, characterized in that: The mixing I is carried out by stirring for more than 30 minutes and then ultrasonically treating for more than 1 hour; The concentration of the graphene oxide in the suspension is 8-30 mg / ml.

3. The preparation method according to claim 1, characterized in that: The coagulation bath solution contains a solvent, and the solvent is ethanol; The concentration of the ionic liquid salt in the coagulation bath solution is 1-2 g / 100 ml ethanol; The ionic liquid salt is 1-ethyl-3-methylimidazolium chloride or 1-ethyl-3-methylimidazolium bromide.

4. The preparation method according to claim 1, characterized in that: When the spinning is advanced, the ambient temperature is between 5 and 70° C.; the diameter of the syringe selected for the spinning is 0.4 to 0.9 mm.

5. The preparation method according to claim 1, characterized in that: The reducing solution is a stannous chloride aqueous solution with a mass fraction greater than 1.5%, or an ascorbic acid aqueous solution with a mass fraction greater than 2%, or a hydroiodic acid solution with a mass fraction greater than 10%.

6. The preparation method according to claim 1, characterized in that: The ambient temperature when reducing the nonwoven fabric is in the range of 30~80℃, and the reduction time is 2~24h; The freeze-drying conditions are a temperature of -60°C to -40°C and a pressure of 10Pa to 90Pa.

7. The preparation method according to claim 1, characterized in that: The vacuum impregnation time needs to be 2h~24h.

8. The composite phase-change nonwoven fabric obtained by any one of the preparation methods of claims 1 to 7.

9. The use of the composite phase change nonwoven fabric according to claim 8, characterized in that: The composite phase-change nonwoven fabric is used as a heat storage and temperature-regulating phase-change material, and maintains the temperature for 2 to 6 hours in the temperature range of 20 to 38°C.