Ultrahigh-temperature ceramic honeycomb and application thereof in methanol-to-olefin process in coal chemical industry
By optimizing the substrate and filter membrane components and processes of ultra-high temperature ceramic honeycombs, and using the method of sintering at a lower temperature in the air atmosphere, the problems of high production costs and insufficient filtration accuracy of existing ceramic honeycombs are solved, and the efficient micron level is achieved Filtration effect and stability are suitable for coal chemical methanol to olefin process.
Patent Information
- Application Number
- CN202411180404.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-12-06
AI Technical Summary
The production process conditions of the existing ultra-high temperature ceramic honeycombs are high, including vacuum conditions and high sintering temperature, resulting in high production costs and traditional materials cannot meet the needs of fine filtration at high temperatures.
Adopt the improved ultra-high temperature ceramic honeycomb process, including the optimization of component of the substrate and filter membrane, the filter membrane is coated by the wetting method, and the sintering temperature is carried out in the air atmosphere, reducing the process conditions requirements, using silicon carbide and Molei Materials such as stone form a honeycomb structure with a multi-channel wall-oriented fluid model.
It realizes low-temperature sintering in air atmosphere, reduces production costs, ensures the stability and filtration accuracy of the finished product, can effectively intercept the micron-level catalyst fine powder, the filtration accuracy reaches 0.3 micron, and the yield rate is high, and there is almost no cracking and Deformation.
Smart Images

Figure CN119080526A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to an ultra-high temperature ceramic honeycomb and application thereof in a coal chemical methanol to olefin process, belonging to the technical field of coal chemical production. Background Art
[0002] At present, the three-cyclone and four-cyclone equipment at the rear end of the methanol-to-olefin reactor and regenerator cannot completely separate the catalyst dust. Under normal circumstances, the dust removal efficiency of the cyclone dust collector can reach about 80% to 95% for particles with a particle size greater than 5 microns, while for fine dust with a particle size less than 5 microns, its capture efficiency will be reduced accordingly. Therefore, it is necessary to cooperate with suitable high-temperature filters to meet the process conditions, and the core material of the high-temperature filter needs to maintain a stable fine filtering effect at high temperatures, and traditional metal or ceramic fibers cannot meet the requirements.
[0003] The Chinese invention patent with the authorization announcement number CN116655388B discloses an ultra-high temperature ceramic honeycomb, including a substrate and a filter membrane. The filter membrane is sprayed on the substrate by plasma spraying technology, and finally the sprayed filter membrane layer is microwave dried and then sintered in a vacuum sintering furnace at 1600-1700°C. However, this solution has high process conditions, such as sintering under vacuum conditions and high sintering temperature requirements, resulting in high production costs. Therefore, how to change the production process and reduce the process conditions and production costs in actual production has become an urgent problem to be solved. Summary of the invention
[0004] Technical purpose: In order to overcome the deficiencies in the prior art, the present invention provides an ultra-high temperature ceramic honeycomb, improves the processing technology, meets the fine filtration requirements under ultra-high temperature conditions, and can be applied in the coal chemical methanol to olefin process.
[0005] Technical solution: To achieve the above-mentioned purpose, the ultra-high temperature ceramic honeycomb disclosed in the present invention includes a substrate and a filter membrane. The components and mass fractions of the substrate are as follows: 90-100 parts of silicon carbide; 0.3-0.5 parts of dispersant; 12-18 parts of pore-forming agent; 3.2-5 parts of kaolin; 0.8-1.2 parts of surfactant; 2.3-3.5 parts of lubricant; 35-40 parts of water; the components and proportions of the filter membrane are as follows: 90-100 parts of mullite; 12-15 parts of ceramic binder; 6-9 parts of stabilizer; 2-4.5 parts of dispersant; 5.5-9 parts of defoaming agent; 80-90 parts of water; the filter membrane is coated on the substrate by an infiltration method.
[0006] Furthermore, the dispersant is one of ethylene glycol, dextrin, fatty acid soaps, and polyols; the pore former is one of graphite, starch, synthetic resin, methyl cellulose, carboxymethyl cellulose, and polyvinyl alcohol; the surfactant is one of polyethylene glycol, sodium fatty acid, and polyethers; and the lubricant is one of glycerol, sorbitol, and pentaerythritol.
[0007] Furthermore, the stabilizer is one of calcium stearate, sodium stearate, magnesium stearate, and aluminum stearate; and the defoaming agent is silicone oil or dimethyl silicone oil.
[0008] Furthermore, the substrate is configured as a multi-channel wall flow fluid model, that is, a honeycomb structure, one side of the substrate is provided with air inlet holes, the other side of the substrate is provided with air outlet holes, and the air inlet holes and the air outlet holes are arranged alternately.
[0009] The method for making an ultra-high temperature ceramic honeycomb comprises the following steps:
[0010] S1: adding the pore former and water into a kneader and mixing for 20 to 30 minutes;
[0011] S2: adding the silicon carbide, dispersant, kaolin and lubricant into a kneader, controlling the temperature within 25-40° C., and kneading for 30-40 minutes;
[0012] S3: adding the surfactant and kneading for 10 to 15 minutes;
[0013] S4: After the mixed material is sealed and settled for 12 to 18 hours, it is poured into an extruder for extrusion molding, and the finished product is transferred to an oven for drying at 60 to 80° C. until the weight no longer decreases;
[0014] S5: Transfer to a kiln for firing, and sinter at 1400-1500°C for 1.5-2h in an air atmosphere to form a base material with a honeycomb structure;
[0015] S6: mixing the components of the filter membrane in a ball mill to form a mixed slurry, adding the mixed slurry to silicon carbide grinding balls, and grinding until a uniform and stable slurry is formed;
[0016] S7: transferring the slurry to a storage tank, and applying the mixed slurry to the surface of the flow channel inside the air inlet hole of the substrate by an infiltration method;
[0017] S8: After the liquid material is dried, it is transferred to a drying oven and dried at 60-80°C until the weight no longer decreases;
[0018] S9: The finished product is transferred to a kiln for firing. In an air atmosphere, it is sintered at 1200-1300°C for 1-1.5 hours to finally form an ultra-high temperature ceramic honeycomb.
[0019] Ultra-high temperature ceramic filter element, including ultra-high temperature ceramic honeycomb.
[0020] Application of ultra-high temperature ceramic filter elements in the methanol to olefins process in coal chemical industry.
[0021] The technical solution of the present invention has at least the following beneficial effects:
[0022] 1. The ultra-high temperature ceramic honeycomb of the present invention is sintered in an air atmosphere at a relatively low sintering temperature, thereby reducing process condition requirements and saving processing costs.
[0023] 2. The present invention ensures that the mixed materials are uniform and stable through the optimization of the substrate, filter membrane components and processes. The sintered finished filter honeycomb has a high yield rate, almost no cracking and deformation problems, and can effectively intercept micron-level catalyst fine powder, with a filtration accuracy of up to 0.3 microns. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 is a schematic diagram of the substrate structure;
[0025] Figure 2 It is a front view of a honeycomb support structure;
[0026] Figure 3 It is a left view of a honeycomb support structure;
[0027] Figure 4 This is an electron microscope picture of the collection of ultra-high temperature filtered honeycomb fine powder of the present invention;
[0028] Figure 5 This is a curve diagram of particle size analysis of fine powder intercepted by the ultra-high temperature filtration honeycomb of the present invention.
[0029] In the figure, 1. air inlet; 2. air outlet; 3. hole wall; 4. support frame; 5. embedded groove; 6. vent; 7. air duct. DETAILED DESCRIPTION
[0030] The following is combined with Figure 1 To Attachment Figure 5 The principles and features of the present invention are described, and the examples given are only used to explain the present invention, not to limit the scope of the present invention.
[0031] The ultra-high temperature ceramic honeycomb comprises a substrate and a filter membrane coated on the substrate.
[0032] Example 1: The components and mass fractions of the substrate and the filter membrane are as follows:
[0033] Substrate: 95 parts of silicon carbide, 0.4 parts of dispersant, 15 parts of pore former, 4 parts of kaolin, 1 part of surfactant, 3 parts of lubricant, and 37 parts of water. The dispersant is ethylene glycol, the pore former is graphite, the surfactant is polyethylene glycol, and the lubricant is glycerol.
[0034] Filter membrane: 95 parts of mullite, 13 parts of ceramic binder, 7 parts of stabilizer, 3 parts of dispersant, 7.5 parts of defoamer, and 85 parts of water. The stabilizer is calcium stearate, the dispersant is ethylene glycol, and the defoamer is silicone oil.
[0035] Example 2: The components and mass fractions of the substrate and the filter membrane are as follows:
[0036] Base material: 90 parts of silicon carbide, 0.3 parts of dispersant, 12 parts of pore former, 3.2 parts of kaolin, 0.8 parts of surfactant, 2.3 parts of lubricant, and 35 parts of water. Among them, the dispersant is dextrin, the pore former is starch, the surfactant is sodium fatty acid, and the lubricant is sorbitol.
[0037] Filter membrane: 90 parts of mullite, 12 parts of ceramic binder, 6 parts of stabilizer, 2 parts of dispersant, 5.5 parts of defoamer, and 80 parts of water. The stabilizer is sodium stearate, the dispersant is dextrin, and the defoamer is silicone oil.
[0038] Example 3: The components and mass fractions of the substrate and the filter membrane are as follows:
[0039] Base material: 100 parts of silicon carbide, 0.5 parts of dispersant, 18 parts of pore former, 5 parts of kaolin, 1.2 parts of surfactant, 3.5 parts of lubricant, and 40 parts of water. The dispersant is fatty acid soap, the pore former is synthetic resin, the surfactant is polyether, and the lubricant is pentaerythritol.
[0040] Filter membrane: 100 parts of mullite; 15 parts of ceramic binder; 9 parts of stabilizer; 4.5 parts of dispersant; 9 parts of defoamer; 90 parts of water. Among them, the stabilizer is magnesium stearate, the dispersant is fatty acid soap, and the defoamer is dimethyl silicone oil.
[0041] like Figure 1 As shown, the substrate is set as a multi-channel wall flow fluid model, that is, a honeycomb structure, an air inlet 1 is set on one side of the substrate, and an air outlet 2 is set on the other side, the air inlet 1 and the air outlet 2 are arranged alternately, a hole wall 3 is formed between the air inlet 1 and the air outlet 2, and the filter membrane is coated on the flow channel surface of the air inlet 1. When in use, the gas to be filtered enters from the air inlet 1, the gas passes through the filter membrane and the hole wall 3 and flows out from the air outlet 2, and the fine dust is intercepted on the filter membrane.
[0042] Example 4: The substrate and filter membrane components in Example 1, Example 2 and Example 3 are respectively operated according to the following production steps to produce an ultra-high temperature ceramic honeycomb.
[0043] S1: Add pore former and water into a kneader and mix for 20-30 minutes;
[0044] S2: Add silicon carbide, dispersant, kaolin and lubricant into a kneader, control the temperature within 25-40°C, and knead for 30-40 minutes;
[0045] S3: Add surfactant and knead for 10-15 minutes;
[0046] S4: After the mixed material is sealed and settled for 12 to 18 hours, it is poured into an extruder for extrusion molding, and the finished product is transferred to an oven for drying at 60 to 80° C. until the weight no longer decreases;
[0047] S5: Transfer to a kiln for firing, and sinter at 1400-1500°C for 1.5-2h in an air atmosphere to form a base material with a honeycomb structure;
[0048] S6: mixing the components of the filter membrane in a ball mill to form a mixed slurry, adding the mixed slurry to silicon carbide grinding balls, and grinding until a uniform and stable slurry is formed;
[0049] S7: transferring the slurry to a storage tank, and applying the mixed slurry to the surface of the flow channel inside the air inlet hole 1 of the substrate by an infiltration method;
[0050] S8: After the liquid material is dried, it is transferred to a drying oven and dried at 60-80°C until the weight no longer decreases;
[0051] S9: The finished product is transferred to a kiln for firing. In an air atmosphere, it is sintered at 1200-1300°C for 1-1.5 hours to finally form an ultra-high temperature ceramic honeycomb.
[0052] Since the sintering conditions are air atmosphere and the sintering temperature is relatively low, the ultra-high temperature ceramic honeycomb sintered using the above process steps will hardly have cracking and deformation problems, ensuring the qualified rate of the finished products. After testing, the qualified rate is over 99.5%.
[0053] Example 5: The ultra-high temperature ceramic honeycomb prepared in Example 4 is embedded into a support body to form a high temperature ceramic filter element. Figure 2 and Figure 3 The figure shows a schematic diagram of a honeycomb support structure, including a support frame 4, a groove 5 is provided on the support frame 4, and a vent 6 is provided at one end of the support frame 4. The ultra-high temperature ceramic honeycomb is embedded in the groove 5 to form a high temperature ceramic filter element, and an air passage 7 is also provided between the bottom wall of the support frame 4 and the ultra-high temperature ceramic honeycomb. The filtered gas passes through the ultra-high temperature ceramic honeycomb and then through the air passage 7 and then is discharged from the vent 6 to complete the gas filtration.
[0054] Example 6: The ultra-high temperature ceramic filter element in Example 5 is applied to the coal chemical methanol to olefin process. The ultra-high temperature ceramic filter element is installed in the high temperature filter, and the high temperature filter is connected to the three-rotor and four-rotor equipment at the rear end of the methanol to olefin reactor and the regenerator. This meets the fine filtering requirements of high-temperature gases above 400 degrees, and the filtering accuracy can reach 0.3um. The dust removal efficiency for dust above 0.3um can reach 99.5%.
[0055] The filter element made of the substrate and filter membrane in Example 1 and the ultra-high temperature honeycomb manufactured in the process steps of Example 4 was subjected to filtration test. Figure 4 The electron microscope image of the fine powder collected on the filter membrane shows that the ultra-high temperature ceramic honeycomb of the present invention effectively intercepts the particles. The fine powder intercepted by the on-site high temperature filter device is then analyzed using a laser particle size distribution analyzer. The relevant experimental data are shown in Figure 5 Among them, curve A is the particle size distribution curve, and curve B is the particle size ratio curve of fine powder. It can be seen that the filtration accuracy of the ultra-high temperature ceramic honeycomb of the present invention can reach 0.3 microns.
[0056] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. An ultra-high temperature ceramic honeycomb, comprising a substrate and a filter membrane, characterized in that: The substrate components and mass fractions are as follows: Silicon carbide 90-100 parts; Dispersant 0.3-0.5 parts; 12 to 18 parts of pore-forming agent; 3.2-5 parts of kaolin; Surfactant 0.8-1.2 parts; 2.3-3.5 parts of lubricant; 35-40 parts of water; The components and proportions of the filtration membrane are as follows: Mullite 90-100 parts; Ceramic binder 12-15 parts; 6-9 parts of stabilizer; 2 to 4.5 parts of dispersant; Defoaming agent 5.5-9 parts; 80-90 parts of water; The filter membrane is coated on the substrate by an infiltration method.
2. The ultra-high temperature ceramic honeycomb according to claim 1, characterized in that: The dispersant is one of ethylene glycol, dextrin, fatty acid soaps, and polyols; the pore former is one of graphite, starch, synthetic resin, methyl cellulose, carboxymethyl cellulose, and polyvinyl alcohol; the surfactant is one of polyethylene glycol, sodium fatty acid, and polyethers; and the lubricant is one of glycerol, sorbitol, and pentaerythritol.
3. The ultra-high temperature ceramic honeycomb according to claim 2, characterized in that: The stabilizer is one of calcium stearate, sodium stearate, magnesium stearate and aluminum stearate; the defoaming agent is silicone oil or dimethyl silicone oil.
4. The ultra-high temperature ceramic honeycomb according to claim 3, characterized in that: The substrate is configured as a multi-channel wall flow fluid model, i.e., a honeycomb structure. One side of the substrate is provided with air inlet holes (1), and the other side of the substrate is provided with air outlet holes (2). The air inlet holes (1) and the air outlet holes (2) are arranged in an alternating manner.
5. The method for manufacturing the ultra-high temperature ceramic honeycomb according to any one of claims 1 to 4, characterized in that: The production steps include: S1: adding the pore former and water into a kneader and mixing for 20 to 30 minutes; S2: adding the silicon carbide, dispersant, kaolin and lubricant into a kneader, controlling the temperature within 25-40° C., and kneading for 30-40 minutes; S3: adding the surfactant and kneading for 10 to 15 minutes; S4: After the mixed material is sealed and settled for 12 to 18 hours, it is poured into an extruder for extrusion molding, and the finished product is transferred to an oven for drying at 60 to 80° C. until the weight no longer decreases; S5: Transfer to a kiln for firing, and sinter at 1400-1500°C for 1.5-2h in an air atmosphere to form a base material with a honeycomb structure; S6: mixing the components of the filter membrane in a ball mill to form a mixed slurry, adding the mixed slurry to silicon carbide grinding balls, and grinding until a uniform and stable slurry is formed; S7: transferring the slurry to a storage tank, and applying the mixed slurry to the surface of the inner flow channel of the air inlet hole (1) of the substrate by an infiltration method; S8: After the liquid material is dried, it is transferred to a drying oven and dried at 60-80°C until the weight no longer decreases; S9: The finished product is transferred to a kiln for firing. In an air atmosphere, it is sintered at 1200-1300°C for 1-1.5 hours to finally form an ultra-high temperature ceramic honeycomb.
6. An ultra-high temperature ceramic filter element, comprising the ultra-high temperature ceramic honeycomb as claimed in any one of claims 1 to 4.
7. Application of the ultra-high temperature ceramic filter element described in claim 6 in the methanol to olefins process of coal chemical industry.
Citation Information
Patent Citations
Ultra-high temperature ceramic honeycomb and its application in silicon powder collection in polycrystalline silicon process
CN116655388B
Fiber-reinforced ceramic filter element and preparation method thereof
CN104387113A
Method for preparing porous ceramic filter membrane by low-temperature sintering
CN104587846A
Catalytic ceramic filter tube and preparation method
CN105107310A
Ultrahigh-temperature ceramic honeycomb and application thereof in silicon powder collection of polycrystalline silicon process