A high-fit composite sodium hyaluronate repair patch and preparation method thereof

Through the preparation of a high-fitting load film, combined with sodium hyaluronate, the problems of weak deformation ability and low compatibility of the carrier material are solved, achieving high fit and improving the repair effect, promoting skin healing and avoiding the need for essence. fluid loss.

CN116270255BActive Publication Date: 2024-10-18HAERBIN FUERSITE BIOLOGY ENG CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202310110728.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-14
Publication Date
2024-10-18
Estimated Expiration
2043-02-14

AI Technical Summary

Technical Problem

The carrier material of the essence in the prior art has weak deformation ability, resulting in poor fit with irregular skin surfaces, and the essence has low compatibility and is prone to dripping, affecting the repair effect.

Method used

Using the preparation method of high-adherence load film, (S)-(+)-glycerol acetone is substituted and ring-opened by 2-bromopropionyl bromide to generate the addition product of hydroxyl and decanoic acid, and reacts with L-proline Amino acid ester derivatives and tert-butoxycarbonyl L-valine undergo amidation and elimination reactions to form a peptide-based polymer film, which is combined with sodium hyaluronate to prepare a repair essence, which improves the elasticity and biocompatibility of the carrier.

Benefits of technology

It improves the fit and repair effect of the repair patch, enhances the retention ability and ductility of the essence, promotes skin healing, and effectively avoids the loss of active ingredients.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004076667880000151
    Figure BDA0004076667880000151
Patent Text Reader

Abstract

The invention discloses a high-fit composite sodium hyaluronate repair patch and a preparation method thereof, and belongs to the technical field of preparations for medical, dental or dressing. The invention includes the preparation of a repair essence and the repair essence impregnating a high-fit load film, the high-fit load film is subjected to ring opening after substitution by (S)-(+)-glycerol acetone with 2-bromopropionyl bromide, the hydroxyl generated by the ring opening is added with decanoic acid to obtain an addition reaction product, the bromine group in the addition reaction product is amidated with L-proline ester derivatives and tert-butyloxycarbonyl L-valine, and the amino group formed by the elimination reaction undergoes a substitution reaction, and the obtained product is polymerized with N-isopropylacrylamide to form a film. The repair essence of the present invention has excellent effect, good compatibility between the carrier material and the essence, the effective active ingredient can be effectively maintained for a long time, and the product is safe and effective.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of medical, dental or cosmetic preparations, and in particular to a high-fit composite sodium hyaluronate repair patch and a preparation method thereof. Background Art

[0002] Sodium hyaluronate is a type of glucuronic acid with gemstone effects. It can improve the microcirculation of blood in the skin and nutrient absorption, help maintain normal metabolism, and play an anti-wrinkle role. Sodium hyaluronate can promote the regeneration of damaged skin by promoting the proliferation and differentiation of epidermal cells and scavenging oxygen free radicals.

[0003] Chinese patent CN107468538A discloses a medical repair patch and a preparation method thereof, comprising a mask cloth and a medicinal solution soaked in the mask cloth; the medicinal solution component comprises, by volume, 0.05% to 0.35% of sodium hyaluronate with a molecular weight of 1,000 to 9,000 Da, 0.08% to 0.40% of sodium hyaluronate with a molecular weight of 800,000 to 1.6 million Da, and 0.05% to 0.06% of sodium hyaluronate with a molecular weight of 1.8 million to 2.5 million Da. .20%, preservative 0.01%~0.10%, thickener 0.05%~0.30%, the balance is water for injection; or sodium hyaluronate with a molecular weight of 0.10,000~0.90,000 Da 0.05%~0.35%, sodium hyaluronate with a molecular weight of 800,000~1.6 million Da 0.08%~0.50%, preservative 0.01%~0.10%, thickener 0.05%~0.40%, the balance is water for injection; the invention is used to treat acne.

[0004] Chinese patent CN113332175A provides a medical wet repair patch, including a nutrient solution and a mask paper soaked in the nutrient solution; wherein the nutrient solution is composed of a mixture of component A, component B and component C; component A, calculated by the total mass percentage of the nutrient solution, is: 2-6% butylene glycol, 2-6% glycerol, 0.5-2% carbomer, 1-4% hydroxyethyl cellulose, 0.01-1% disodium ethylenediaminetetraacetic acid, 0.1-1% sodium propylparaben, 0.1-1% flavoring agent and deionized water; component B is: 0.02-0.2% triethanolamine; component C is: 0.5-2% recombinant human type III collagen, 0.05-2% sodium hyaluronate and 1-6% β-glucan; the medical wet repair patch has the functions of moisturizing and repairing. It can be applied in the fields of medical plastic surgery and cosmetic makeup, such as the repair and maintenance of the skin after medical plastic surgery such as laser, photorejuvenation, freezing, high frequency, grinding, and facelift; the treatment of skin injuries such as depressed scars, skin erythema, atrophy, sunburn, and burns caused by acne or trauma.

[0005] In the prior art, the carrier materials of essences are mostly non-woven fabrics or polymer films. Although they are widely available and easy to carry, they generally have the technical problems of weak deformation ability and poor adhesion to irregular skin surfaces. In addition, the above-mentioned carrier materials mainly absorb essences by increasing the specific surface area, and are not highly compatible with the essences. When used, there may be defects such as excessive essences and easy dripping, which affects the repair effect of the essences. Summary of the invention

[0006] In view of the above-mentioned defects of the prior art, the problem to be solved by the present invention is to provide a high-fit composite sodium hyaluronate repair patch and a preparation method thereof.

[0007] The invention discloses a method for preparing a high-fit composite sodium hyaluronate repair patch, which comprises the preparation of a repair essence and the soaking of a high-fit load film with the repair essence.

[0008] A method for preparing a high-fit composite sodium hyaluronate repair patch comprises the following steps:

[0009] S1. Mix 0.5-1.5wt% sodium hyaluronate, 0.2-0.6wt% carbomer, 0.2-0.8wt% sodium polyglutamate, 1.6-3.0wt% glycerol, 0.01-0.1wt% preservative and the remainder of deionized water, and stir at 40-55° C. for 0.5-2.0h to obtain a repair essence;

[0010] S2. Immerse the high-fitting load film in the repair essence, take it out after the repair essence is soaked, and package it after sterilization to obtain a high-fitting composite sodium hyaluronate repair patch.

[0011] Preferably, the sodium hyaluronate in step S1 is prepared by mixing high molecular weight sodium hyaluronate and low molecular weight sodium hyaluronate in a mass ratio of 1:(0.8-1.5); wherein the molecular weight of the high molecular weight sodium hyaluronate is 1.2-1.8 million Daltons, and the molecular weight of the low molecular weight sodium hyaluronate is 100,000-300,000 Daltons.

[0012] Preferably, the molecular weight of the sodium polyglutamate in step S1 is 50,000 to 100,000 Daltons.

[0013] Preferably, the stirring rate in step S1 is 800-1200 rpm.

[0014] Preferably, in step S2, the solid-liquid mass ratio of the high-fitting loading membrane to the repair essence is 1:(5.5-8.0).

[0015] The invention adopts (S)-(+)-glycerol acetone acetonide to undergo ring opening after substitution with 2-bromopropionyl bromide, and the hydroxyl group generated by the ring opening is added with decanoic acid to obtain an addition reaction product, and the bromine group in the addition reaction product is amidated with an L-proline ester derivative and tert-butyloxycarbonyl L-valine, and then an amino group formed by an elimination reaction undergoes a substitution reaction, and the product is polymerized with N-isopropylacrylamide to form a film, thereby obtaining a high-fitting load film.

[0016] The above-mentioned high-fitting loading membrane exhibits excellent elastic properties and good biocompatibility. The high-fitting loading membrane is a peptide-based polymer containing L-proline ester derivatives and tert-butyloxycarbonyl L-valine structures. Compared with traditional non-woven materials, it has greater advantages in skin compatibility and promoting the healing of skin damage. In the high-fitting loading membrane, due to the interaction of dipole-dipole, hydrogen bonds, charge transfer complexes and van der Waals forces between polymer chains, it has the characteristics of two cross-linked monomers. In the process of polymerization and film formation, the molecular helices between the monomers penetrate and entangle with each other to form a non-ionic hydrophilic, highly elastic membrane. Hydroxyl and ether oxygen bonds promote the formation of hydrogen bonds with water molecules, increasing the membrane's ability to retain essence; the flexibility of ether oxygen bonds and other bonds gives the membrane excellent ductility.

[0017] The structure of the peptide-based polymer of the high-fitting loading membrane is similar to the glycosaminoglycan structure of sodium hyaluronate, and the two have good binding properties. After loading the repair essence, the effective active ingredients can be effectively maintained on the membrane for a long time and are not easily wasted and lost due to factors such as water molecules, which helps to improve the repair effect of the repair patch.

[0018] Preferably, the preparation method of the high-fitting load film is as follows:

[0019] M1. Mix (S)-(+)-glycerol acetone and dichloromethane uniformly, add a catalyst and 2-bromopropionyl bromide to the mixture, mix again and then carry out a first substitution reaction; after the first substitution reaction, add hydrochloric acid to the substituted crude product, mix and extract with dichloromethane, collect the organic phase, wash the organic phase with saturated brine, dry, and remove dichloromethane by reduced pressure distillation to obtain a first substitution reaction product for standby use;

[0020] M2, mixing the first substitution reaction product and acetic acid aqueous solution uniformly, and then performing a ring-opening reaction; after the ring-opening reaction is completed, the ring-opening crude product is extracted with dichloromethane, and the organic phase is collected, and the organic phase is dried and distilled under reduced pressure to remove dichloromethane to obtain a ring-opening reaction product for standby use;

[0021] M3, the ring-opening reaction product, the catalyst and dichloromethane are mixed uniformly, and then decanoic acid is added to carry out an addition reaction; after the addition reaction is completed, the filtrate is collected by filtration, and the dichloromethane is removed by reduced pressure distillation to obtain an addition reaction product for standby use;

[0022] M4, mixing L-proline ester derivative, tert-butyloxycarbonyl L-valine and N,N-dimethylformamide uniformly, then adding a catalyst to carry out an amidation reaction; after the amidation reaction is completed, the product is subjected to reduced pressure distillation to remove N,N-dimethylformamide, and the residue is collected; the residue is washed with water and dried to obtain an amidation reaction product for standby use;

[0023] M5, mixing the amidation reaction product, the catalyst and anhydrous ethanol uniformly, and then performing an elimination reaction; after the elimination reaction, removing the anhydrous ethanol by distillation, washing with a saturated sodium bicarbonate aqueous solution, and drying to obtain an elimination reaction product for standby use;

[0024] M6, uniformly mixing the elimination reaction product, the addition reaction product and acetone, and then performing a second substitution reaction; after the second substitution reaction is completed, removing the acetone by vacuum distillation, washing with water, and drying to obtain a second substitution reaction product for standby use;

[0025] M7. Evenly mix the second substitution reaction product, N-isopropylacrylamide, initiator and deionized water to obtain a prepolymer solution; place the prepolymer solution in a mold and perform a polymerization reaction under anaerobic conditions; after the polymerization reaction is completed, dry and demold to obtain a high-fitting load film.

[0026] Specifically, the preparation method of the highly conformable loading membrane is as follows, in parts by weight:

[0027] M1, take 2.95-3.85 parts of (S)-(+)-glycerol acetone and 125-175 parts of dichloromethane and mix them evenly, add 4.50-5.90 parts of triethylamine and 6.75-8.80 parts of 2-bromopropionyl bromide to the mixture, mix them evenly again and then carry out a first substitution reaction; after the first substitution reaction is completed, add 90-120 parts of hydrochloric acid to the substituted crude product, mix and extract with 75-100 parts of dichloromethane, collect the organic phase, wash the organic phase with saturated brine, dry, and remove dichloromethane by reduced pressure distillation to obtain the first substitution reaction product, and set aside;

[0028] M2, taking another 4.75-6.15 parts of the first substitution reaction product and mixing them evenly with 60-75 parts of acetic acid aqueous solution, and then performing a ring-opening reaction; after the ring-opening reaction is completed, the ring-opening crude product is extracted with 75-100 parts of dichloromethane, and the organic phase is collected, and the organic phase is dried and distilled under reduced pressure to remove dichloromethane to obtain a ring-opening reaction product for standby use;

[0029] M3, take 1.75-2.30 parts of the ring-opening reaction product, 0.25-0.40 parts of 4-dimethylaminopyridine, 3.55-4.60 parts of N,N-dicyclohexylcarbodiimide and 100-150 parts of dichloromethane and mix them evenly, then add 2.95-3.85 parts of decanoic acid and carry out addition reaction; after the addition reaction is completed, collect the filtrate by filtration, remove dichloromethane by reduced pressure distillation, and obtain the addition reaction product for standby use;

[0030] M4, taking 2.20-3.50 parts of L-proline ester derivative, 2.80-3.70 parts of tert-butyloxycarbonyl L-valine and 75-100 parts of N, N-dimethylformamide and mixing them evenly, then adding 2.50-3.25 parts of 1-ethyl-(3-dimethylaminopropyl) carbodiimide hydrochloride, 1.75-2.30 parts of 1-hydroxybenzotriazole and 2.10-2.75 parts of N-methylmorpholine, and performing an amidation reaction; after the amidation reaction is completed, the product is subjected to reduced pressure distillation to remove N, N-dimethylformamide, and the residue is collected; the residue is washed with water and dried to obtain an amidation reaction product, which is used for standby;

[0031] M5, taking another 2.15-2.80 parts of the amidation reaction product, 1.15-1.50 parts of trifluoroacetic acid and 50-75 parts of anhydrous ethanol and mixing them evenly, and then performing an elimination reaction; after the elimination reaction, the anhydrous ethanol is removed by distillation, and the product is washed with a saturated sodium bicarbonate aqueous solution and dried to obtain an elimination reaction product for standby use;

[0032] M6, taking another 2.20-2.85 parts of the elimination reaction product, 2.35-3.10 parts of the addition reaction product and 75-100 parts of acetone and mixing them evenly, and then performing a second substitution reaction; after the second substitution reaction is completed, removing the acetone by vacuum distillation, washing with water, and drying to obtain a second substitution reaction product for standby use;

[0033] M7, take another 2.25-2.95 parts of the second substitution reaction product, 1.15-1.50 parts of N-isopropylacrylamide, 0.01-0.03 parts of azobisisobutyronitrile and 20-40 parts of deionized water and mix them evenly to obtain a prepolymer solution; place the prepolymer solution in a mold, and perform polymerization reaction under nitrogen protection; after the polymerization reaction is completed, dry and demold to obtain a high-fitting load film.

[0034] Preferably, the first substitution reaction in step M1 is carried out in two stages. The reactants are first reacted at a temperature of 0 to 4° C. for 1.5 to 4.0 h; and then reacted at 20 to 30° C. for 6 to 18 h.

[0035] Preferably, the concentration of the hydrochloric acid in step M1 is 0.5-1.0 mol / L.

[0036] Preferably, the concentration of the acetic acid aqueous solution in step M2 is 60-80 wt %

[0037] Preferably, the temperature of the ring-opening reaction in step M2 is 55-70° C., and the reaction time is 1.5-5.0 h.

[0038] Preferably, the temperature of the addition reaction in step M3 is 20-35° C., and the reaction time is 6-12 h.

[0039] Preferably, the L-proline ester derivative in step M4 is any one of L-proline methyl ester, L-proline isopropyl ester and L-proline benzyl ester.

[0040] Preferably, the temperature of the amidation reaction in step M4 is 25-40° C., and the reaction time is 8-24 h.

[0041] Preferably, the temperature of the elimination reaction in step M5 is 25-35° C., and the reaction time is 0.5-2.0 h.

[0042] Preferably, the temperature of the second substitution reaction in step M6 is 10-20° C., and the reaction time is 6-18 h.

[0043] Preferably, the polymerization reaction temperature in step M7 is 65-80° C., and the reaction time is 4-12 hours.

[0044] On the basis of being in accordance with the common sense in the art, the above-mentioned preferred conditions can be arbitrarily combined to obtain the preferred embodiments of the present invention.

[0045] The introduction and functions of some raw materials in the formula of the present invention are as follows:

[0046] Sodium hyaluronate: chemical formula is (C 14 H 20 NO 11 Na) n It is an inherent component in the human body. It is a kind of glucuronic acid. It has no species specificity. It is widely present in tissues and organs such as the placenta, amniotic fluid, lens, articular cartilage, and skin dermis. It is distributed in the cytoplasm and interstitial matrix, and plays a lubricating and nourishing role on the cells and cell organs contained therein. Moisturizing is the most important role of sodium hyaluronate in cosmetics. Compared with other moisturizers, the relative humidity of the surrounding environment has less effect on its moisturizing properties.

[0047] Sodium polyglutamate: The carboxyl group of the glutamic acid unit side chain of polyglutamic acid is ionized to form an anionic carboxylate (COO - ) and then combined with sodium ions to form a product. Sodium polyglutamate has excellent water solubility and is a natural moisturizing ingredient. It is now widely used as a moisturizing raw material for cosmetics.

[0048] Beneficial effects of the present invention:

[0049] Compared with the prior art, the present invention provides a method for preparing a high-fit composite sodium hyaluronate repair patch, including the preparation of a repair essence and the penetration of the repair essence into a high-fit load film. Among them, the present invention uses (S)-(+)-glycerol acetone to undergo ring opening after substitution with 2-bromopropionyl bromide, and the hydroxyl group generated by the ring opening is added with decanoic acid to obtain an addition reaction product, and the bromine group in the addition reaction product undergoes amidation with L-proline ester derivatives and tert-butyloxycarbonyl L-valine, and then the amino group formed by the elimination reaction undergoes a substitution reaction, and the product is polymerized with N-isopropylacrylamide to form a film.

[0050] Compared with the prior art, the carrier of the repair patch prepared and used in the present invention is a peptide-based polymer containing L-proline ester derivatives and tert-butyloxycarbonyl L-valine structure, which has greater advantages in skin compatibility and promoting the healing of skin damage compared to traditional non-woven materials. The structure of the peptide-based polymer of the high-fitting loading membrane is similar to the glycosaminoglycan structure of sodium hyaluronate, and the two have good binding properties. After loading the repair essence, the effective active ingredients can be effectively maintained on the membrane for a long time, and are not easily wasted and lost due to the influence of factors such as water molecules, which helps to improve the repair effect of the repair patch.

[0051] Compared with the prior art, the load film of the repair patch of the present invention exhibits excellent elastic properties and good biocompatibility. In the high-fit load film, due to the interaction of dipole-dipole, hydrogen bonds, charge transfer complexes and van der Waals forces between polymer chains, it has the characteristics of two cross-linked monomers. In the process of polymerization into film, the molecular helices between the monomers penetrate and entangle with each other to form a non-ionic hydrophilic, highly elastic film. Hydroxyl and ether oxygen bonds promote the formation of hydrogen bonds with water molecules, increasing the film's ability to retain essence; the flexibility of ether oxygen bonds and other bonds gives the film excellent ductility. DETAILED DESCRIPTION

[0052] The present invention is further described below by way of examples, but the present invention is not limited to the scope of the examples. The experimental methods in the following examples without specifying specific conditions are carried out according to conventional methods and conditions, or selected according to the product specifications.

[0053] Some raw material parameters in the comparative examples and embodiments of the present invention are as follows:

[0054] High molecular weight sodium hyaluronate, 1.5 million Daltons, provided by Shanghai Lianmai Bioengineering Co., Ltd.;

[0055] Low molecular weight sodium hyaluronate, 200,000 Daltons, provided by Shandong Runxin Biological Co., Ltd.;

[0056] Sodium polyglutamate, 100,000 Daltons, provided by Shanghai Yuanye Biotechnology Co., Ltd.;

[0057] Carbomer 940, pharmaceutical grade, provided by Xi'an Jinxiang Pharmaceutical Excipients Co., Ltd.;

[0058] Sodium propylparaben, pharmaceutical grade, provided by Xi'an Tianzheng Pharmaceutical Excipients Co., Ltd.;

[0059] Chitosan mask base fabric, brand: BOLREUS, item number: 01, provided by Shenzhen Xinzhongjie Nonwoven Fabric Co., Ltd.

[0060] Example 1

[0061] A high-fit composite sodium hyaluronate repair patch is prepared by the following method:

[0062] S1. 1.0 wt% sodium hyaluronate, 0.4 wt% carbomer 940, 0.5 wt% sodium polyglutamate, 2.3 wt% glycerol, 0.05 wt% sodium propylparaben and the remainder of deionized water were mixed, and the mixture was stirred at 50° C. and 1000 rpm for 1.5 h to obtain a repair essence;

[0063] S2. Immerse the high-fitting load film in the repair essence, wherein the solid-liquid mass ratio of the high-fitting load film to the repair essence is 1:7; take it out after the repair essence is soaked, and package it after sterilization to obtain a high-fitting composite sodium hyaluronate repair patch.

[0064] The sodium hyaluronate is prepared by mixing high molecular weight sodium hyaluronate and low molecular weight sodium hyaluronate in a mass ratio of 1:1.5.

[0065] The preparation method of the high-fitting load film is as follows:

[0066] M1, take 2.95kg (S) - (+) - glycerol acetone acetone and 125kg dichloromethane and mix them evenly, add 4.50kg triethylamine and 6.75kg 2-bromopropionyl bromide to the mixture, mix them evenly again and then carry out the first substitution reaction, the reaction is carried out in two stages, the reactants are first reacted at a temperature of 0 ° C for 3h; then reacted at 25 ° C for 12h; after the first substitution reaction is completed, 90kg hydrochloric acid with a concentration of 1mol / L is added to the substituted crude product, and after mixing, it is extracted with 75kg dichloromethane, and the organic phase is collected, and the organic phase is washed with saturated brine, dried, and distilled under reduced pressure to remove dichloromethane to obtain the first substitution reaction product, which is set aside;

[0067] M2, take another 4.75kg of the first substitution reaction product and mix it evenly with 60kg of 80wt% acetic acid aqueous solution, and then carry out a ring-opening reaction, the temperature of the ring-opening reaction is 65°C, and the reaction time is 3.5h; after the ring-opening reaction, the ring-opening crude product is extracted with 75kg of dichloromethane, and the organic phase is collected, and the organic phase is dried and distilled under reduced pressure to remove dichloromethane to obtain a ring-opening reaction product for standby use;

[0068] M3, take another 1.75kg of the ring-opening reaction product, 0.25kg of 4-dimethylaminopyridine, 3.55kg of N,N-dicyclohexylcarbodiimide and 100kg of dichloromethane and mix them evenly, then add 2.95kg of decanoic acid and carry out addition reaction, the temperature of the addition reaction is 30°C, and the reaction time is 9h; after the addition reaction is completed, the filtrate is collected by filtration, and the dichloromethane is removed by reduced pressure distillation to obtain the addition reaction product, which is set aside;

[0069] M4, 3.50 kg of L-proline ester derivative, 2.80 kg of tert-butyloxycarbonyl L-valine and 75 kg of N, N-dimethylformamide were mixed uniformly, and then 2.50 kg of 1-ethyl-(3-dimethylaminopropyl) carbodiimide hydrochloride, 1.75 kg of 1-hydroxybenzotriazole and 2.10 kg of N-methylmorpholine were added to carry out an amidation reaction, the temperature of the amidation reaction was 40 ° C, and the reaction time was 18 hours; after the amidation reaction was completed, the product was subjected to reduced pressure distillation to remove N, N-dimethylformamide, and the residue was collected; the residue was washed with water and dried to obtain an amidation reaction product for standby use;

[0070] M5, take another 2.15kg of the amidation reaction product, 1.15kg of trifluoroacetic acid and 50kg of anhydrous ethanol and mix them evenly, then carry out elimination reaction, the temperature of the elimination reaction is 30°C, and the reaction time is 1.5h; after the elimination reaction is completed, the anhydrous ethanol is removed by distillation, and the saturated sodium bicarbonate aqueous solution is washed and dried to obtain the elimination reaction product for standby use;

[0071] M6, take another 2.20kg of the elimination reaction product, 2.35kg of the addition reaction product and 75kg of acetone and mix them evenly, then carry out a second substitution reaction, the reaction temperature is 10°C, and the reaction time is 12h; after the second substitution reaction is completed, remove the acetone by vacuum distillation, wash with water, and dry to obtain a second substitution reaction product for standby use;

[0072] M7. Take another 2.25 kg of the second substitution reaction product, 1.15 kg of N-isopropylacrylamide, 0.01 kg of azobisisobutyronitrile and 20 kg of deionized water and mix them evenly to obtain a prepolymer solution; after placing the prepolymer solution in a mold, perform a polymerization reaction under nitrogen protection at a temperature of 75°C and a reaction time of 8 hours; after the polymerization reaction is completed, dry and demold to obtain a high-fitting load film.

[0073] The L-proline ester derivative is L-proline benzyl ester.

[0074] Example 2

[0075] This example is basically the same as Example 1, except that the L-proline ester derivative is L-proline methyl ester, and the amount used is 2.20 kg.

[0076] Example 3

[0077] This example is basically the same as Example 1, except that the L-proline ester derivative is L-proline isopropyl ester, and the amount used is 2.65 kg.

[0078] Example 4

[0079] A high-fit composite sodium hyaluronate repair patch is prepared by the following method:

[0080] S1. 1.0 wt% sodium hyaluronate, 0.4 wt% carbomer 940, 0.5 wt% sodium polyglutamate, 2.3 wt% glycerol, 0.05 wt% sodium propylparaben and the remainder of deionized water were mixed, and the mixture was stirred at 50° C. and 1000 rpm for 1.5 h to obtain a repair essence;

[0081] S2. Immerse the high-fitting load film in the repair essence, wherein the solid-liquid mass ratio of the high-fitting load film to the repair essence is 1:7; take it out after the repair essence is soaked, and package it after sterilization to obtain a high-fitting composite sodium hyaluronate repair patch.

[0082] The sodium hyaluronate is prepared by mixing high molecular weight sodium hyaluronate and low molecular weight sodium hyaluronate in a mass ratio of 1:1.5.

[0083] The preparation method of the high-fitting load film is as follows:

[0084] M1, take 3.85kg (S) - (+) - glycerol acetone acetone and 175kg dichloromethane and mix them evenly, add 5.90kg triethylamine and 8.80kg 2-bromopropionyl bromide to the mixture, mix them evenly again and then carry out the first substitution reaction, the reaction is carried out in two stages, the reactants are first reacted at a temperature of 0 ° C for 3h; then reacted at 25 ° C for 12h; after the first substitution reaction is completed, 120kg hydrochloric acid with a concentration of 1mol / L is added to the substituted crude product, and after mixing, it is extracted with 100kg dichloromethane, and the organic phase is collected, and the organic phase is washed with saturated brine, dried, and distilled under reduced pressure to remove dichloromethane to obtain the first substitution reaction product, which is set aside;

[0085] M2, taking another 6.15kg of the first substitution reaction product and mixing it with 75kg of 80wt% acetic acid aqueous solution, and then performing a ring-opening reaction, the temperature of the ring-opening reaction is 65°C, and the reaction time is 3.5h; after the ring-opening reaction is completed, the ring-opening crude product is extracted with 100kg of dichloromethane, and the organic phase is collected, and the organic phase is dried and distilled under reduced pressure to remove dichloromethane to obtain a ring-opening reaction product for standby use;

[0086] M3, take another 2.30kg of the ring-opening reaction product, 0.40kg of 4-dimethylaminopyridine, 4.60kg of N,N-dicyclohexylcarbodiimide and 150kg of dichloromethane and mix them evenly, then add 3.85kg of decanoic acid and carry out addition reaction, the temperature of the addition reaction is 30°C, and the reaction time is 9h; after the addition reaction is completed, the filtrate is collected by filtration, and the dichloromethane is removed by reduced pressure distillation to obtain the addition reaction product, which is set aside;

[0087] M4, take 3.50kg L-proline benzyl ester, 3.70kg tert-butyloxycarbonyl L-valine and 100kg N, N-dimethylformamide and mix them evenly, then add 3.25kg 1-ethyl-(3-dimethylaminopropyl) carbodiimide hydrochloride, 2.30kg 1-hydroxybenzotriazole and 2.75kg N-methylmorpholine, and carry out amidation reaction, the temperature of amidation reaction is 40°C, and the reaction time is 18h; after the amidation reaction is completed, the product is subjected to reduced pressure distillation to remove N, N-dimethylformamide, and the residue is collected; the residue is washed with water and dried to obtain an amidation reaction product, which is set aside;

[0088] M5, take another 2.80kg of the amidation reaction product, 1.50kg of trifluoroacetic acid and 75kg of anhydrous ethanol and mix them evenly, then carry out elimination reaction, the temperature of the elimination reaction is 30°C, and the reaction time is 1.5h; after the elimination reaction is completed, the anhydrous ethanol is removed by distillation, and the saturated sodium bicarbonate aqueous solution is washed and dried to obtain the elimination reaction product for standby use;

[0089] M6, take another 2.85kg of the elimination reaction product, 3.10kg of the addition reaction product and 100kg of acetone and mix them evenly, then carry out a second substitution reaction, the reaction temperature is 10°C, and the reaction time is 12h; after the second substitution reaction is completed, remove the acetone by vacuum distillation, wash with water, and dry to obtain a second substitution reaction product for standby use;

[0090] M7. Take another 2.95 kg of the second substitution reaction product, 1.50 kg of N-isopropylacrylamide, 0.03 kg of azobisisobutyronitrile and 40 kg of deionized water and mix them evenly to obtain a prepolymer solution; after placing the prepolymer solution in a mold, perform a polymerization reaction under nitrogen protection at a temperature of 75°C and a reaction time of 8 hours; after the polymerization reaction is completed, dry and demold to obtain a high-fitting load film.

[0091] Comparative Example 1

[0092] A sodium hyaluronate repair patch is prepared by the following method:

[0093] S1. 1.0 wt% sodium hyaluronate, 0.4 wt% carbomer 940, 0.5 wt% sodium polyglutamate, 2.3 wt% glycerol, 0.05 wt% sodium propylparaben and the remainder of deionized water were mixed, and the mixture was stirred at 50° C. and 1000 rpm for 1.5 h to obtain a repair essence;

[0094] S2. Immerse the chitosan mask base fabric in the repair essence solution, wherein the solid-liquid mass ratio of the chitosan mask base fabric to the repair essence solution is 1:7; take out the base fabric after the repair essence solution has penetrated through it, and package it after sterilization to obtain a sodium hyaluronate repair patch.

[0095] The sodium hyaluronate is prepared by mixing high molecular weight sodium hyaluronate and low molecular weight sodium hyaluronate in a mass ratio of 1:1.5.

[0096] Test Example 1

[0097] The tensile properties of the high-fit load film of the high-fit composite sodium hyaluronate repair patch and its liquid retention performance compared with the control example were tested. The tensile performance test was carried out with reference to the specific methods and steps in GB / T1040.3-2006 "Determination of Tensile Properties of Plastics Part 3: Test Conditions for Films and Sheets". The test specimen is a type 5 specimen, and based on the use requirements of the present invention, the results are characterized by elongation at break. The liquid retention performance test of the high-fit load film prepared in each embodiment and the chitosan mask base fabric used in the control example was measured using a WPT-304 moisture permeability tester. The temperature of the moisture permeability tester is 37°C and the humidity is 65%. The test is carried out according to the test method in Section 3.2.9 of the literature (Mao Wenxuan. Mask Base Fabric Performance Test and Evaluation [D]. Shanghai: Donghua University, 2021.). The test results of the tensile properties and liquid retention properties of the high-fit load film are shown in Table 1.

[0098] Table 1:

[0099] project Elongation at break (%) Fluid retention (%) Example 1 657 93.7 Example 2 578 80.9 Example 3 612 85.2 Comparative Example 1 / 64.8

[0100] Test Example 2

[0101] The biosafety test of the high-fit load membrane used in the present invention includes an in vitro cytotoxicity test and a hemolysis test. The in vitro cytotoxicity test is carried out with reference to the specific methods and steps in GB / T 16886.5-2017 "Biological Evaluation of Medical Devices Part 5: In Vitro Cytotoxicity Test", the extraction conditions are a) conditions, the test method is a direct contact test, and the test cell line is American Type Culture Collection CCL1 (NCTC clone 929); the qualitative grading of the cytotoxic morphology of the extract is shown in Table 2. The hemolysis test is carried out with reference to the specific methods and steps in YY / T 1651.1-2019 "Hemolysis Test for Medical Devices Part 1: Material-Mediated Hemolysis Test", and the test adopts a direct contact method. The test results of the in vitro cytotoxicity test and the hemolysis test are shown in Table 3.

[0102] Table 2:

[0103]

[0104] Table 3:

[0105] project Degree of reaction Hemolysis rate (%) Example 1 none 0.3 Example 2 none 0.5 Example 3 none 0.4 Example 4 none 0.3

[0106] According to the provisions of YY / T 1651.1-2019, 0%<hemolysis rate<2% is considered as non-hemolysis. It can be seen from the above test results that none of the examples showed in vitro cytotoxicity and hemolysis.

[0107] Based on the results of the above test examples, it can be seen that the present invention has good elasticity and biocompatibility. The reason for this result may be that the high-fitting load membrane is a peptide-based polymer containing L-proline ester derivatives and tert-butyloxycarbonyl L-valine structures, which has greater advantages in skin compatibility and promoting the healing of skin damage compared to traditional non-woven materials. In the high-fitting load membrane, due to the interaction of dipole-dipole, hydrogen bonds, charge transfer complexes and van der Waals forces between polymer chains, it has the characteristics of two cross-linked monomers. In the process of polymerization and film formation, the molecular helices between the monomers penetrate and entangle with each other to form a non-ionic hydrophilic, highly elastic membrane. Hydroxyl and ether oxygen bonds promote the formation of hydrogen bonds with water molecules, increasing the membrane's ability to retain essence; the flexibility of ether oxygen bonds and other bonds gives the membrane excellent ductility. The structure of the peptide-based polymer of the high-fitting loading membrane is similar to the glycosaminoglycan structure of sodium hyaluronate, and the two have good binding properties. After loading the repair essence, the effective active ingredients can be effectively maintained on the membrane for a long time and are not easily wasted and lost due to factors such as water molecules, which helps to improve the repair effect of the repair patch.

Claims

1. A method for preparing a high-fit composite sodium hyaluronate repair patch, characterized in that: The steps include: S1. Mix 0.5-1.5wt% sodium hyaluronate, 0.2-0.6wt% carbomer, 0.2-0.8wt% sodium polyglutamate, 1.6-3.0wt% glycerol, 0.01-0.1wt% preservative and the remainder of deionized water, and stir at 40-55° C. for 0.5-2.0h to obtain a repair essence; S2, immersing the high-fitting load film in the repair essence, taking it out after the repair essence is soaked, and packaging it after sterilization to obtain a high-fitting composite sodium hyaluronate repair patch; The preparation method of the highly conformable loading membrane is as follows, in parts by weight: M1, take 2.95-3.85 parts of (S)-(+)-glycerol acetone and 125-175 parts of dichloromethane and mix them evenly, add 4.50-5.90 parts of triethylamine and 6.75-8.80 parts of 2-bromopropionyl bromide to the mixture, mix them evenly again and then carry out a first substitution reaction; after the first substitution reaction is completed, add 90-120 parts of hydrochloric acid to the substituted crude product, mix and extract with 75-100 parts of dichloromethane, collect the organic phase, wash the organic phase with saturated brine, dry, and remove dichloromethane by reduced pressure distillation to obtain the first substitution reaction product, and set aside; M2, taking another 4.75-6.15 parts of the first substitution reaction product and mixing them evenly with 60-75 parts of acetic acid aqueous solution, and then performing a ring-opening reaction; after the ring-opening reaction is completed, the ring-opening crude product is extracted with 75-100 parts of dichloromethane, and the organic phase is collected, and the organic phase is dried and distilled under reduced pressure to remove dichloromethane to obtain a ring-opening reaction product for standby use; M3, take 1.75-2.30 parts of the ring-opening reaction product, 0.25-0.40 parts of 4-dimethylaminopyridine, 3.55-4.60 parts of N,N-dicyclohexylcarbodiimide and 100-150 parts of dichloromethane and mix them evenly, then add 2.95-3.85 parts of decanoic acid and carry out addition reaction; after the addition reaction is completed, collect the filtrate by filtration, remove dichloromethane by reduced pressure distillation, and obtain the addition reaction product for standby use; M4, taking 2.20-3.50 parts of L-proline ester derivative, 2.80-3.70 parts of tert-butyloxycarbonyl L-valine and 75-100 parts of N, N-dimethylformamide and mixing them evenly, then adding 2.50-3.25 parts of 1-ethyl-(3-dimethylaminopropyl) carbodiimide hydrochloride, 1.75-2.30 parts of 1-hydroxybenzotriazole and 2.10-2.75 parts of N-methylmorpholine, and performing an amidation reaction; after the amidation reaction is completed, the product is subjected to reduced pressure distillation to remove N, N-dimethylformamide, and the residue is collected; the residue is washed with water and dried to obtain an amidation reaction product, which is used for standby; M5, taking another 2.15-2.80 parts of the amidation reaction product, 1.15-1.50 parts of trifluoroacetic acid and 50-75 parts of anhydrous ethanol and mixing them evenly, and then performing an elimination reaction; after the elimination reaction, the anhydrous ethanol is removed by distillation, and the product is washed with a saturated sodium bicarbonate aqueous solution and dried to obtain an elimination reaction product for standby use; M6, taking another 2.20-2.85 parts of the elimination reaction product, 2.35-3.10 parts of the addition reaction product and 75-100 parts of acetone and mixing them evenly, and then performing a second substitution reaction; after the second substitution reaction is completed, removing the acetone by vacuum distillation, washing with water, and drying to obtain a second substitution reaction product for standby use; M7, taking 2.25-2.95 parts of the second substitution reaction product, 1.15-1.50 parts of N-isopropylacrylamide, 0.01-0.03 parts of azobisisobutyronitrile and 20-40 parts of deionized water and mixing them evenly to obtain a prepolymer solution; placing the prepolymer solution in a mold, and performing a polymerization reaction under nitrogen protection; after the polymerization reaction is completed, drying and demolding are performed to obtain a high-fitting load film; The first substitution reaction in step M1 is carried out in two stages. The reactants are first reacted at a temperature of 0 to 4°C for 1.5 to 4.0 hours; then reacted at 20 to 30°C for 6 to 18 hours; the temperature of the ring-opening reaction in step M2 is 55 to 70°C, and the reaction time is 1.5 to 5.0 hours; the temperature of the addition reaction in step M3 is 20 to 35°C, and the reaction time is 6 to 12 hours; The temperature of the amidation reaction in step M4 is 25-40° C., and the reaction time is 8-24 h; The temperature of the elimination reaction in step M5 is 25-35° C., and the reaction time is 0.5-2.0 h; The L-proline ester derivative in step M4 is any one of L-proline methyl ester, L-proline isopropyl ester, and L-proline benzyl ester; The temperature of the second substitution reaction in step M6 is 10-20° C., and the reaction time is 6-18 h; The polymerization reaction temperature in step M7 is 65-80° C., and the reaction time is 4-12 hours.

2. The method for preparing the high-fit composite sodium hyaluronate repair patch according to claim 1, characterized in that: The sodium hyaluronate described in step S1 is prepared by mixing high molecular weight sodium hyaluronate and low molecular weight sodium hyaluronate in a mass ratio of 1: (0.8-1.5); wherein the molecular weight of the high molecular weight sodium hyaluronate is 1.2-1.8 million Daltons, and the molecular weight of the low molecular weight sodium hyaluronate is 100,000-300,000 Daltons; and the molecular weight of the sodium polyglutamate is 50,000-100,000 Daltons.

3. A high-fit composite sodium hyaluronate repair patch, characterized in that: The method is prepared by the method according to any one of claims 1 to 2.

Citation Information

Patent Citations

  • A medical restoration patch and a preparing method thereof

    CN107468538A

  • Medical wet repair patch

    CN113332175A

  • Glycerol levulinate ketals and their use

    CN101346067A

  • Biological functionalization degradable polyester and preparation method thereof

    CN102532502A