A catalyst for degrading organic pollutants in wastewater and its preparation method and application
Through the combination of cobalt single atom supported nitrogen-doped porous carbon catalyst and peroxymonosulfate, the problem of degradation of organic pollutants in industrial wastewater is solved, efficient catalytic oxidation effect and stability are achieved, secondary pollution is avoided, and Simplified process flow.
Patent Information
- Application Number
- CN202310292423.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-23
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2043-03-23
AI Technical Summary
Existing technology is difficult to effectively degrade organic pollutants in industrial wastewater, especially toxic substances that are difficult to degrade naturally such as phenols and dyes, and the solid waste generated during industrial treatment cannot be rationally utilized, resulting in secondary pollution problems.
A nitrogen-doped porous carbon catalyst supported by a cobalt single atom is used. By mixing chitosan with a transition metal salt, a nitrogen source and a pore-forming agent and then calcining it at high temperature, a catalyst with high catalytic performance is prepared for use with peroxymonosulfuric acid. Salt binding treats organic pollutants in wastewater.
The catalyst can effectively degrade organic pollutants in wastewater, improve catalytic oxidation activity, reduce the leaching rate of metal atoms, improve stability and regeneration capacity, avoid secondary pollution, and achieve low cost and easy operation for industrial application. sex.
Smart Images

Figure CN116273126B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of wastewater treatment, and in particular to a catalyst for degrading organic pollutants in wastewater, and a preparation method and application thereof. Background Art
[0002] With the continuous development of chemical industry and urbanization, the water pollution problem caused by the large-scale discharge of industrial wastewater is one of the environmental problems that urgently need to be solved. Water is an important resource for human survival. Although the amount of water on the earth is huge, very little of it can be directly used by people for production and life. The freshwater resources on the earth only account for 2.5% of its total amount, and most of the freshwater resources exist in the icebergs in the North and South Poles and the alpine glaciers on land that are difficult to use. The amount that humans can really use only accounts for 0.26% of the total water on the earth. Especially in recent years, due to the rapid development of industries such as chemical and pharmaceutical industries, there are still a large number of toxic substances that are difficult to degrade naturally in the various wastewaters discharged, such as phenols, antibiotics, dyes, etc. These polluted wastewaters cause great harm to the ecosystem and human health through the natural circulation system. In addition, humans are also facing environmental and climate change problems caused by excessive emissions of greenhouse gases. The diversity of industrial production makes the nature of the drainage pollution generated also complicated. Multi-stage treatment processes are often used in industrial wastewater treatment. Almost all multi-stage wastewater treatment processes involve coagulation and flocculation steps, but the solid waste after flocculation is often not properly utilized, which leads to the problem of secondary pollution.
[0003] In addition, with the development of advanced oxidation technology for treating wastewater pollutants in recent years, the advanced oxidation method based on permonosulfate (PMS) has received widespread attention. Compared with the traditional Fenton system, PMS has stronger oxidation ability and a wider pH range, so it has great application potential. The role of the catalyst in this reaction is very critical. The development of a catalyst with simple preparation, low cost and high catalytic performance is of great significance for the practical application of this reaction.
[0004] Through detection, no patent publication documents related to the patent application of the present invention have been found. Summary of the invention
[0005] The purpose of the present invention is to overcome the deficiencies in the prior art and provide a catalyst for degrading organic pollutants in wastewater and a preparation method and application thereof.
[0006] The technical solution adopted by the present invention to solve its technical problem is:
[0007] A method for preparing a catalyst for degrading organic pollutants in wastewater comprises the following steps:
[0008] Adding chitosan to the first wastewater to obtain floccules, mixing the floccules, transition metal salts, nitrogen sources and pore-forming agents uniformly and freeze-drying the mixture to obtain a precursor, and calcining the precursor at 700-900° C. under the protection of an inert gas to obtain the catalyst, i.e., nitrogen-doped porous carbon supported by a single cobalt atom;
[0009] Wherein, the first wastewater is wastewater containing at least one dye organic pollutant, and the pore-forming agent is polystyrene microspheres.
[0010] Furthermore, the catalyst comprises pores with pore diameters of 40-80 nm and 160-200 nm.
[0011] Furthermore, the organic pollutant is selected from at least one of methyl orange, azo ruby red, new carmine, orange II and Coomassie brilliant blue; preferably, the organic pollutant is methyl orange.
[0012] Further, the transition metal salt is selected from at least one of cobalt chloride hexahydrate and cobalt nitrate hexahydrate; preferably cobalt chloride hexahydrate;
[0013] The nitrogen source is selected from at least one of melamine, urea and dicyandiamide, preferably melamine;
[0014] Alternatively, the weight ratio of the chitosan to the organic pollutant is 4-6:1, preferably 5:1;
[0015] and / or, the weight ratio of the flocculant to the transition metal salt is 4.2-62.5:1, preferably 10.4:1;
[0016] and / or, the weight ratio of the pore former to the flocculant is 6-12:1, preferably 8:1;
[0017] And / or, the weight ratio of the transition metal salt to the nitrogen source is 0.05-0.4:1, preferably 0.16:1.
[0018] Furthermore, the specific preparation steps of the precursor are as follows:
[0019] The flocculants are added to an acid solution, and after being fully dissolved, a transition metal salt and a nitrogen source are added, and after stirring for at least 8 hours, a pore-forming agent is added, and after stirring for at least 8 hours, freeze-dried to obtain a precursor;
[0020] Alternatively, the specific preparation steps of the catalyst are as follows:
[0021] The precursor is calcined at 700-900° C. for 1.5-2.5 hours and then naturally cooled to room temperature to obtain the catalyst; wherein the heating rate is 1.5-2.5° C. / min.
[0022] Further, the acid solution is glacial acetic acid;
[0023] The precursor is calcined at 800° C. for 2 hours and then naturally cooled to room temperature to obtain the catalyst; wherein the heating rate is 2° C. / min.
[0024] Furthermore, the weight ratio of the flocculants to the glacial acetic acid is 0.417:1.
[0025] The catalyst is prepared by the preparation method described above.
[0026] Use of the catalyst as described above in degrading organic pollutants in wastewater.
[0027] The method for degrading organic pollutants in wastewater using the catalyst as described above comprises the following steps:
[0028] The catalyst is added to the second wastewater containing organic pollutants, and after being evenly dispersed, peroxymonosulfate is added and stirred;
[0029] Wherein, the organic pollutant includes at least one of bisphenol A, phenol, rhodamine B, methyl orange and 2,4-dichlorophenol;
[0030] The weight ratio of the catalyst to the organic pollutant is 0.2-0.8:1, preferably 0.5:1;
[0031] The mass concentration of the peroxymonosulfate in the second wastewater is 200-500 mg / L, preferably 300 mg / L.
[0032] The advantages and positive effects achieved by the present invention are:
[0033] 1. The catalyst of the present invention uses chitosan, a safe and non-toxic natural polymer biomass, as a flocculant, and treats the secondary pollutants generated after treating wastewater through pyrolysis activation, converting them into nitrogen-doped porous carbon catalysts with high catalytic oxidation degradation activity, which has a dual significance for wastewater treatment.
[0034] 2. In the catalyst of the present invention, the metal atoms and nitrogen atoms are in a strong coordination state, which avoids the leaching of metal atoms and makes the metal atoms in a single-atom dispersion state, thereby improving the utilization rate of metal atoms, reducing costs, and improving the stability of the catalyst.
[0035] 3. The catalyst of the present invention does not require a water washing process during its preparation, has the advantages of simple operation, low cost, high catalyst yield, wide operating range, long service life, strong universality, and easy industrialization.
[0036] 4. When the catalyst of the present invention is used for oxidation treatment of wastewater pollutants, it can optimize the mass transfer effect, increase the contact area with the pollutants, and enhance the catalytic oxidation activity. Moreover, the stable macroporous structure is not easily blocked by reaction intermediates, and therefore has excellent regeneration ability.
[0037] 5. The catalyst of the present invention uses solid flocculants in wastewater as a carbon source, and adds transition metal salts and nitrogen sources for modification, and adds pore-forming agents, and synthesizes transition metal single-atom nitrogen-doped three-dimensional ordered macroporous carbon materials through a one-step high-temperature calcination method. The abundant nitrogen atoms in the material can anchor transition metal atoms, avoid the aggregation of transition metal atoms during the calcination process, and ensure that transition metal atoms can be evenly loaded in the porous carbon material. The transition metal exists in the form of atomic active sites, which have higher catalytic activity and stability than nanoparticle active sites. In addition, the three-dimensional ordered macroporous structure of the material fully exposes the active sites. When it is used as a catalyst for treating wastewater pollutants by advanced oxidation method, it can optimize the mass transfer effect, increase the contact area with pollutants, and enhance the catalytic oxidation activity. The stable macroporous structure is not easily blocked by reaction intermediates, which is beneficial to the regeneration of the catalyst.
[0038] In addition, chitosan as a flocculant can provide abundant amino and hydroxyl groups and has polycationic properties, so it has a good adsorption effect on organic pollutants. Chitosan is a natural polymer biomass, safe and non-toxic, and will not cause secondary pollution. Secondary pollutants produced after industrial flocculant treatment of wastewater are often not further utilized. The floccules produced after using chitosan as a flocculant to treat wastewater are converted into nitrogen-doped porous carbon catalysts with high catalytic oxidation degradation activity through pyrolysis activation treatment, which has dual significance for wastewater treatment.
[0039] 6. The method of the present invention selects polystyrene microspheres as pore-forming agents, which can interact with the flocculation substrate through charge, so that the polystyrene microspheres can be evenly embedded in the modified flocculation substrate, and can form a uniform and orderly three-dimensional macroporous structure after calcination. No water washing process is required, the operation is simple, the cost is low, and the catalyst yield is high.
[0040] 7. The method of the present invention selects cobalt as a transition metal source, which has a wide range of sources, and the standard redox potential of cobalt (1.82V) is very close to the standard redox potential of peroxymonosulfate (1.75V), so the catalyst loaded with cobalt has a better effect of activating peroxymonosulfate. By selecting melamine as a nitrogen source, the nitrogen content is high, the source is wide, the cost is low, and the transition metal atoms can be fully anchored during the calcination process.
[0041] 8. The method of the present invention carbonizes the organic matter in the precursor by controlling the calcination conditions. In addition, the stacked polyethylene microspheres are pyrolyzed to form a three-dimensional macroporous structure with abundant interconnected pores, so that the final catalyst has a large specific surface area, is not easy to collapse, and has a strong regeneration ability.
[0042] 9. The present invention is used to treat organic pollutants in wastewater. The catalyst is used as an oxidation catalyst to treat wastewater pollutants. It has fully exposed Co single-atom active sites, exhibits high Fenton-like catalytic activity and stability in peroxymonosulfate activation and degradation of organic pollutants.
[0043] The first wastewater after flocculation and removal of floccules can be directly used as the second wastewater, or the wastewater without flocculation can be used as the second wastewater. When the second wastewater is the first wastewater after flocculation and removal of floccules, the floccules in the first wastewater can be used to prepare the catalyst of the present application, and the prepared catalyst is used as a catalyst for treating the second wastewater by oxidation, thereby realizing closed-loop utilization. BRIEF DESCRIPTION OF THE DRAWINGS
[0044] Figure 1 It is a curve diagram of the flocculation effect of different chitosan dosages and pH values in the present invention;
[0045] Figure 2 This is a diagram showing the flocculation effects of azo ruby red, new carmine, orange II and Coomassie brilliant blue at different pH values in the present invention;
[0046] Figure 3 The morphology of the polystyrene microspheres and the catalyst Co-NC-PS in the present invention;
[0047] Figure 4 The morphology diagram of the catalyst under different dosages of polystyrene microspheres in the present invention;
[0048] Figure 5 The isothermal adsorption-desorption curves and pore size distribution diagrams of the catalysts at different polystyrene microsphere dosages in the present invention;
[0049] Figure 6 are X-ray diffraction (XRD) patterns of different catalysts in the present invention;
[0050] Figure 7 X-ray diffraction (XRD) diagrams of catalysts with different Co contents in the present invention;
[0051] Figure 8 : are Raman spectra of different catalysts in the present invention;
[0052] Fig. 9 It is the XPS graph of the catalyst with different Co contents in the present invention;
[0053] Fig.10 TEM morphology of catalysts with different Co contents in the present invention. DETAILED DESCRIPTION
[0054] The present invention will be further described below in conjunction with the embodiments. The following embodiments are descriptive rather than restrictive, and the protection scope of the present invention cannot be limited by the following embodiments.
[0055] The various experimental operations involved in the specific embodiments are all routine techniques in the art. For parts not specially annotated in this document, ordinary technicians in the art can implement them by referring to various commonly used reference books, scientific and technological literature or related instructions, manuals, etc. before the filing date of this invention.
[0056] A method for preparing a catalyst for degrading organic pollutants in wastewater comprises the following steps:
[0057] Adding chitosan to the first wastewater to obtain floccules, mixing the floccules, transition metal salts, nitrogen sources and pore-forming agents uniformly and freeze-drying the mixture to obtain a precursor, and calcining the precursor at 700-900° C. under the protection of an inert gas to obtain the catalyst, i.e., nitrogen-doped porous carbon supported by a single cobalt atom;
[0058] Wherein, the first wastewater is wastewater containing at least one dye organic pollutant, and the pore-forming agent is polystyrene microspheres.
[0059] Preferably, the catalyst comprises pores with pore diameters of 40-80 nm and 160-200 nm.
[0060] Preferably, the organic pollutant is selected from at least one of methyl orange, azo ruby red, new carmine, orange II and Coomassie brilliant blue; preferably, the organic pollutant is methyl orange.
[0061] Preferably, the transition metal salt is selected from at least one of cobalt chloride hexahydrate and cobalt nitrate hexahydrate; preferably cobalt chloride hexahydrate;
[0062] The nitrogen source is selected from at least one of melamine, urea and dicyandiamide, preferably melamine;
[0063] Alternatively, the weight ratio of the chitosan to the organic pollutant is 4-6:1, preferably 5:1;
[0064] and / or, the weight ratio of the flocculant to the transition metal salt is 4.2-62.5:1, preferably 10.4:1;
[0065] and / or, the weight ratio of the pore former to the flocculant is 6-12:1, preferably 8:1;
[0066] And / or, the weight ratio of the transition metal salt to the nitrogen source is 0.05-0.4:1, preferably 0.16:1.
[0067] Preferably, the specific preparation steps of the precursor are as follows:
[0068] The flocculants are added to an acid solution, and after being fully dissolved, a transition metal salt and a nitrogen source are added, and after stirring for at least 8 hours, a pore-forming agent is added, and after stirring for at least 8 hours, freeze-dried to obtain a precursor;
[0069] Alternatively, the specific preparation steps of the catalyst are as follows:
[0070] The precursor is calcined at 700-900° C. for 1.5-2.5 hours and then naturally cooled to room temperature to obtain the catalyst; wherein the heating rate is 1.5-2.5° C. / min.
[0071] Preferably, the acid is glacial acetic acid;
[0072] The precursor is calcined at 800° C. for 2 hours and then naturally cooled to room temperature to obtain the catalyst; wherein the heating rate is 2° C. / min.
[0073] Preferably, the weight ratio of the flocculants to the glacial acetic acid is 0.417:1.
[0074] The catalyst is prepared by the preparation method described above.
[0075] Use of the catalyst as described above in degrading organic pollutants in wastewater.
[0076] The method for degrading organic pollutants in wastewater using the catalyst as described above comprises the following steps:
[0077] The catalyst is added to the second wastewater containing organic pollutants, and after being evenly dispersed, peroxymonosulfate is added and stirred;
[0078] Wherein, the organic pollutant includes at least one of bisphenol A, phenol, rhodamine B, methyl orange and 2,4-dichlorophenol;
[0079] The weight ratio of the catalyst to the organic pollutant is 0.2-0.8:1, preferably 0.5:1;
[0080] The mass concentration of the peroxymonosulfate in the second wastewater is 200-500 mg / L, preferably 300 mg / L.
[0081] Specifically, the relevant preparation and detection are as follows:
[0082] The analysis method in the embodiment of the present invention can be as follows:
[0083] The crystal structure was analyzed by high-resolution XRD (Bruker-Nonius D8 Focus).
[0084] The morphology of the catalyst was observed using SEM (instrument model: Hitachi S-4800);
[0085] The specific surface area of the catalyst was tested using BET (instrument model: BJBulider SSA-7000);
[0086] The atomic state was observed using HAADF-STEM (instrument model: JEM-ARM200F);
[0087] The morphology and element distribution of the catalyst were observed using TEM (instrument model: JEOL JEM-2100F).
[0088] X-ray photoelectron spectroscopy (XPS, Thermo Hermo ESCALAB 250XI) was used to characterize the bonding and chemical structure of the materials.
[0089] The cobalt leaching rate and cobalt content of the catalyst were determined by inductively coupled plasma atomic emission spectrometry (ICP-OES, Optima 7300DV, USA).
[0090] The degree of defects in the samples was studied using Raman spectroscopy (Renishaw in Viareflex, 633nm laser).
[0091] The flocculation effect was characterized by UV spectrophotometer (UV 1800PC).
[0092] Example 1
[0093] The preparation method of catalyst 1# is as follows:
[0094] (1) Dissolve 0.05 g of methyl orange in 1 L of deionized water to simulate 50 mg / L of organic pollutant wastewater;
[0095] (2) 0.25 g of chitosan was added to the simulated pollutant wastewater and stirred vigorously until fully mixed to obtain a mixed solution; then 1 mol / L hydrochloric acid solution was slowly added to the mixed solution to adjust the pH to 5, and the stirring was stopped after fully stirring for 30 min, and the mixture was allowed to stand for 12 h; then the supernatant was poured out to obtain about 10 mL of bottom floccules;
[0096] (3) The bottom flocs obtained in step (2) were transferred to a 50 ml beaker, 0.6 g of glacial acetic acid solution was added thereto, heated and stirred at 50 ° C to fully dissolve it, and then 24 mg of CoCl2·6H2O and 0.15 g of melamine were added. After stirring for 12 h and fully mixed, the polystyrene microsphere emulsion was added to the above solution at a mass ratio of polystyrene microspheres to bottom flocs of 8:1, and stirred for 12 h. The obtained liquid was placed in a refrigerator and then freeze-dried in a vacuum freeze dryer at -40 ° C and 10 Pa to obtain a precursor;
[0097] (4) The precursor obtained in step (3) was transferred to a corundum boat and calcined and carbonized in a tubular furnace under a N2 atmosphere. The temperature was raised from room temperature to 800°C and maintained for 2 h, and then naturally cooled to room temperature. The heating rate was 2°C / min. The black sample obtained by calcination was finally collected and was catalyst 1#, denoted as Co-NC-PS.
[0098] The catalytic oxidation process of organic pollutants in wastewater is as follows:
[0099] (1) Prepare 100 mL of 20 ppm bisphenol A solution and ultrasonicate for 30 minutes to simulate organic pollutant wastewater;
[0100] (2) 10 mg of the catalyst was added to the organic pollutant wastewater obtained in step (1), and stirred on a magnetic stirrer for 20 minutes to reach adsorption-desorption equilibrium. Stirring was continued, and 30 mg of permonosulfate was added to the reaction system, and then the timing was quickly started. 0.5 mL of the solution was taken out from the reaction system at 0, 1, 2, 5, 10, 20, 30, 45, and 60 minutes, and then the taken out solution was immediately injected into a screw-capped bottle with 0.5 mL of methanol to quench the reaction.
[0101] (3) A mixed solution containing 70% methanol and 30% deionized water was used as the mobile phase with a flow rate of 1 mL / min. The degradation amount of bisphenol A was measured by a high performance liquid chromatograph (HPLC, Hitachi) with a Supersil ODS-B column. The test results are shown in Table 1.
[0102] (4) The catalyst in the reaction system is recovered and used as a catalyst again to carry out the catalytic oxidation process of steps (1) to (3). The catalyst recovered for the first time is recorded as Co-NC-PS (2nd), and the test results are shown in Table 2. The catalyst recovered for the second time is recorded as Co-NC-PS (3rd), and the test results are shown in Table 3. The catalyst recovered for the third time is recorded as Co-NC-PS (4th), and the test results are shown in Table 4.
[0103] Table 1
[0104]
[0105] Table 2
[0106]
[0107] Table 3
[0108]
[0109]
[0110] Table 4
[0111]
[0112] It can be seen from Tables 1 to 4 that when the catalyst is used for oxidation treatment of wastewater pollutants, it has high catalytic oxidation activity and strong regeneration ability.
[0113] Example 2
[0114] The difference between Example 2 and Example 1 is that during the preparation of the catalyst, the mass ratio of polystyrene microspheres to bottom flocculants is 4:1, and the other conditions are the same, thus obtaining catalyst 2#, which is recorded as Co-NC-PS (4:1);
[0115] The catalyst added in the catalytic oxidation process of organic pollutants in the wastewater is catalyst 2#, and the degradation amount of bisphenol A is measured. The test results are shown in Table 5.
[0116] Table 5
[0117]
[0118] Example 3
[0119] The difference between Example 3 and Example 1 is that during the preparation of the catalyst, the mass ratio of polystyrene microspheres to bottom flocculants is 12:1, and the other conditions are the same, thus obtaining catalyst 3#, which is recorded as Co-NC-PS (12:1);
[0120] The catalyst added in the catalytic oxidation process of organic pollutants in the wastewater is catalyst 3#, and the degradation amount of bisphenol A is measured. The test results are shown in Table 6.
[0121] Table 6
[0122]
[0123]
[0124] From Table 1, Table 5 and Table 6, it can be seen that with Co-NC-PS (4:1) as the catalyst, the BPA degradation rate is 95.1% within 60 minutes. The time for Co-NC-PS (8:1) and Co-NC-PS (12:1) systems to completely degrade BPA is 10 minutes. The results show that the amount of polystyrene microspheres has a great influence on the degradation of BPA.
[0125] Embodiment 4, 5, 6, 7
[0126] The difference between Examples 4, 5, 6 and 7 and Example 1 is that: during the preparation of the catalyst, azo ruby red, new carmine, orange II and Coomassie brilliant blue were added in sequence instead of methyl orange, and the other conditions were the same to obtain catalysts 4#, 5#, 6# and 7#, which were respectively recorded as Co-NC-PS (azo ruby red), Co-NC-PS (new carmine), Co-NC-PS (orange II) and Co-NC-PS (Coomassie brilliant blue);
[0127] The catalyst added in the catalytic oxidation process of organic pollutants in the wastewater is catalyst 3#, and the degradation amount of bisphenol A is measured. The test results are shown in Tables 7 to 10.
[0128] Table 7
[0129]
[0130] Table 8
[0131]
[0132] Table 9
[0133]
[0134] Table 10
[0135]
[0136] The flocculation substrate treated with the above four dyes (azo ruby, new carmine, orange II, Coomassie brilliant blue) was modified and calcined under the same conditions as the above Co-NC-PS to obtain Co-NC-PS (azo ruby), Co-NC-PS (new carmine), Co-NC-PS (orange II) and Co-NC-PS (Coomassie brilliant blue). The performance of the prepared materials in degrading organic pollutants was evaluated. It can be seen that under the catalysis of Co-NC-PS (azo ruby), Co-NC-PS (new carmine), Co-NC-PS (orange II) and Co-NC-PS (Coomassie brilliant blue) systems, bisphenol A can be completely degraded within 10 minutes.
[0137] Embodiments 8, 9, 10, 11, 12
[0138] The difference between Examples 8, 9, 10, 11, and 12 and Example 1 is that during the preparation of the catalyst, the amount of CoCl2·6H2O added was 1.5, 3, 12, 48, and 60 mg, respectively. The other conditions were the same, and catalysts 8#, 9#, 10#, 11#, and 12# were obtained, which were respectively denoted as Co (1.5) -NC-PS, Co (3) -NC-PS, Co (12) -NC-PS, Co (48) -NC-PS, Co (60) -NC-PS;
[0139] The catalyst added in the catalytic oxidation process of organic pollutants in the wastewater is catalyst 7#, and the degradation amount of bisphenol A is measured. The test results are shown in Tables 11 to 15.
[0140] Table 11
[0141]
[0142] Table 12
[0143]
[0144] Table 13
[0145]
[0146] Table 14
[0147]
[0148]
[0149] Table 15
[0150]
[0151] From Table 1, Table 11-18, it can be seen that Co (1.5) -NC-PS, Co (3) -NC-PS, Co (12) -NC-PS, Co-NC-PS, Co (48) -NC-PS and Co (60) The complete degradation time of BPA by Co-NC-PS system was 60min, 45min, 15min, 10min, 20min and 30min respectively. The results showed that the Co atom in Co-NC-PS catalyst may be the main active site for BPA degradation. (X)The reaction rate of the -NC-PS system shows a peak shape with the increase of the amount of Co precursor, and Co-NC-PS has the best catalytic performance.
[0152] Embodiment 13
[0153] The difference between Example 13 and Example 1 is that in the preparation process of the catalyst, urea is used instead of melamine, and the other conditions are the same, to obtain catalyst 13#, denoted as Co-NC-PS (urea);
[0154] The catalyst added in the catalytic oxidation process of organic pollutants in the wastewater is catalyst 14#, and the degradation amount of bisphenol A is measured. The test results are shown in Table 16.
[0155] Table 16
[0156]
[0157] It can be seen from Table 16 that when urea is used instead of melamine as the nitrogen source, the complete degradation time of BPA by the Co-NC-PS (urea) system is 30 min. Melamine as a nitrogen source has a better degradation effect.
[0158] Embodiment 14, 15
[0159] The difference between Examples 14 and 15 and Example 1 is that during the preparation of the catalyst, the calcination temperature is 700°C and 900°C, and the calcination time is 2 h. The other conditions are the same, and catalysts 14# and 15# are obtained, which are respectively recorded as Co-NC-PS (700°C) and Co-NC-PS (900°C);
[0160] The catalysts added in the catalytic oxidation process of organic pollutants in the wastewater are catalysts 14# and 15#. The degradation amount of bisphenol A was measured. The test results are shown in Tables 17-18.
[0161] Table 17
[0162]
[0163] Table 18
[0164]
[0165] It can be seen from Table 1, Table 17 and Table 18 that when the calcination temperatures are 700°C, 800°C and 900°C, the complete degradation time for BPA is 20 min, 10 min and 10 min respectively.
[0166] Example 16
[0167] The difference between Example 16 and Example 1 is that: during the preparation of the catalyst, the amount of melamine added is 300 mg, and the other conditions are the same, to obtain catalyst 16#, denoted as Co-NC-PS (nitrogen source added);
[0168] The catalyst added in the catalytic oxidation process of organic pollutants in the wastewater is catalyst 16#, and the degradation amount of bisphenol A is measured. The test results are shown in Table 19.
[0169] Table 19
[0170]
[0171] It can be seen from Table 1 and Table 19 that when the amount of melamine added is 150 mg and 300 mg, the complete degradation time of BPA is 10 minutes. The addition of excessive melamine does not improve its degradation effect.
[0172] Embodiment 17
[0173] The difference between Example 17 and Example 1 is that during the catalytic oxidation of organic pollutants in wastewater, the amount of catalyst 1# added was 50 mg, and the other conditions were the same. The degradation amount of bisphenol A was measured, and the test results are shown in Table 20.
[0174] Table 20
[0175]
[0176]
[0177] It can be seen from Table 20 that when the added amount of catalyst is 50 mg, the Co-NC-PS system can only degrade 95.3% BPA within 60 min.
[0178] Embodiments 18, 19, and 20
[0179] The difference between Examples 18, 19, and 20 and Example 1 is that: during the catalytic oxidation of organic pollutants in wastewater, 100 mL of 20 ppm rhodamine B solution, phenol solution, and 2,4-dichlorophenol solution were prepared and ultrasonicated for 30 minutes to simulate organic pollutant wastewater;
[0180] The other conditions were the same, and the degradation amounts of phenol solution, rhodamine B solution, and 2,4-dichlorophenol solution were measured. The experimental results are shown in Tables 21-23.
[0181] Table 21
[0182]
[0183] Table 22
[0184]
[0185] Table 23
[0186]
[0187] It can be seen that with Co-NC-PS as a catalyst and permonosulfate as an oxidant, rhodamine B (RhB), phenol and 2,4-dichlorophenol (2,4-dcp) can be completely degraded within 10 min. These results confirm that Co-NC-PS can be used as a catalyst to effectively activate permonosulfate and achieve complete degradation of various dyes and phenolic organic pollutants.
[0188] Embodiment 21
[0189] The difference between Example 21 and Example 1 is that during the catalytic oxidation of organic pollutants in wastewater, the amounts of permonosulfate added were 10 mg, 20 mg and 50 mg respectively, and the other conditions were the same. The degradation amount of bisphenol A was measured, and the test results are shown in Tables 24-26.
[0190] Table 24
[0191]
[0192]
[0193] Table 25
[0194]
[0195] Table 26
[0196]
[0197] It can be seen that as the dosage of peroxymonosulfate increases from 100 mg·L -1 Increase to 300mg·L -1 , the degradation rate of bisphenol A increased significantly, and the k value increased from 0.0315min -1 Significantly increased to 1.290min -1 However, when the persulfate dosage was increased to 500 mg·L -1 When , the degradation efficiency did not increase significantly, indicating that excessive PMS may cause self-quenching of the system and hinder degradation.
[0198] Comparative Example 1
[0199] The difference between Comparative Example 1 and Example 1 is that: during the preparation of the catalyst, no pore-forming agent is added, and the other conditions are the same, to obtain catalyst D1#, denoted as Co-NC;
[0200] The catalyst added in the catalytic oxidation process of organic pollutants in wastewater is catalyst D1#. The degradation amount of bisphenol A is measured. The experimental results are shown in Table 27.
[0201] Table 27
[0202]
[0203]
[0204] It can be seen from Table 27 that with Co-NC as the catalyst, the BPA degradation rate within 60 min was only 16.0%. The results show that the polystyrene microsphere template has a great influence on the degradation of BPA.
[0205] Comparative Example 2
[0206] The difference between Comparative Example 2 and Example 1 is that melamine is not added during the preparation of the catalyst, and the other conditions are the same to obtain catalyst D2#, which is recorded as NPs Co-NC-PS;
[0207] The catalyst added in the catalytic oxidation process of organic pollutants in wastewater is catalyst D2, and the degradation amount of bisphenol A is measured. The experimental results are shown in Table 28. After the catalyst is recovered, its degradation rate of bisphenol A is measured again, and the experimental results are shown in Table 29.
[0208] Table 28
[0209]
[0210] Table 29
[0211]
[0212] After the first cycle, the efficiency of the NPs Co-NC-PS catalyst decreased by more than 70%. In sharp contrast to the NPs Co-NC-PS catalyst, the Co-NC-PS catalyst has good recyclability. Although the degradation rate decreased, 97% of bisphenol A could be removed within 60 minutes after 4 experimental cycles. Atomic absorption spectrometer (AAS) was used to detect the amount of cobalt leached in the solution after the reaction. After the first cycle, the amount of Co leached in the NPs Co-NC-PS system was 2.2 mg·L-1, while the amount of Co leached in the Co-NC-PS system could not be detected after the reaction. It is speculated that the loss of active sites after the reaction may be the main reason for the decrease in the activity of NPsCo-NC-PS. The strong stability of the single-atom Co-NC-PS catalyst is likely to originate from the stabilization of the Co-N4 active sites.
[0213] Comparative Example 3
[0214] The difference between Comparative Example 3 and Example 1 is that: during the preparation of the catalyst, the amount of CoCl2·6H2O added is 0, and the other conditions are the same, and catalyst D3# is obtained, which is recorded as NC-PS;
[0215] The catalyst added in the catalytic oxidation process of organic pollutants in the wastewater is catalyst 7#, and the degradation amount of bisphenol A is measured. The test results are shown in Table 30.
[0216] Table 30
[0217]
[0218] As can be seen from Table 30, the BPA degradation effect using NC-PS as a catalyst reached 66.7% within 60 min, indicating that N-doped carbon has little effect on the activation of PMS.
[0219] It can also be seen from Comparative Examples 1 to 3 and Example 1 that there is a synergistic effect between the transition metal salt, the nitrogen source and the pore-forming agent during the preparation of the catalyst of the present invention, and the transition metal salt, the nitrogen source and the pore-forming agent can synergistically improve the relevant performance of the prepared catalyst.
[0220] In addition, the effects of different chitosan dosages and pH values on flocculation were also determined. Figure 1 As shown, when the chitosan dosage is 250 mg and the flocculation pH is 5, the optimal removal rate can reach 88.9%.
[0221] like Figure 2 As shown, Figure 2 (a) and Figure 2 (b) is the flocculation effect of azo ruby red at different pH values. Figure 2 (c) and Figure 2 (d) shows the flocculation effect of new carmine at different pH values. Figure 2 (e) and Figure 2 (f) is the flocculation effect of Orange II at different pH values. Figure 2 (g) and Figure 2 (h) is the flocculation effect of Coomassie Brilliant Blue at different pH values. It can be seen that the best removal rates of Azo Ruby, New Carmine, Orange II and Coomassie Brilliant Blue at pH = 6 can reach 99.9%, 99.9%, 99.8% and 98.5%, respectively. These results show that chitosan is an excellent dye flocculant.
[0222] like Figure 2 As shown, Figure 3(a) is a scanning electron microscope (SEM) image of polystyrene microspheres (PS), from which it can be seen that the polystyrene microspheres are uniform spheres with a diameter of ~360 nm. The negatively charged PS microspheres on the surface act as structural templates and are electrostatically bonded to the positively charged chitosan polymer (carbon source) through protonated amine groups. In the subsequent pyrolysis process, the modified flocculation substrate is carbonized at 800°C to form nitrogen-doped carbon sheets. In addition, N atoms can anchor Co atoms to the carbon skeleton in the form of Co-NC bonds. Figure 3 (b) also shows that Co-NC-PS exhibits a three-dimensional ordered macroporous structure with abundant pores after high-temperature calcination. The pore diameter is between 160 and 200 nm. As the molten PS spheres shrink during calcination, the macropores formed are smaller than those of the initial template. In addition, the stacked PS microspheres are pyrolyzed to form abundant interconnected pores of about 40-80 nm (see Figure 3 c) In addition, Figure 3 (d) is the transmission electron microscopy (TEM) image of Co-NC-PS. It can be clearly observed that Co-NC-PS presents a three-dimensional hollow structure, and no clusters or nanoparticles are observed. High-angle annular dark field scanning transmission electron microscopy (HAADF-STEM) verifies that the Co atoms ( Figure 3 e, 3f and 3g). Rich Co single atoms (highlights, Figure 3 f) are evenly dispersed on the carbon matrix. The corresponding energy dispersive X-ray spectroscopy (EDS) mapping ( Figure 3 g) shows that Co, C, N, O, and S are uniformly distributed throughout the carbon skeleton, and the presence of a small amount of S atoms in the resulting material also confirms the effective utilization of organic components in simulated dye wastewater.
[0223] like Figure 4 As shown in Figure 2, the effect of the amount of polystyrene microspheres on the morphology and pore structure of porous carbon was further studied. The Co-NC synthesized without PS microsphere template has a block structure and no macroporous structure ( Figure 4 a). The SEM image of Co-NC-PS (4:1) shows that some scattered holes appear on the sample surface due to the removal of the polystyrene microsphere template ( Figure 4 b). As the number of polystyrene microspheres increases, Co-NC-PS exhibits a three-dimensional ordered macroporous (3DOM) structure with abundant pores ( Figure 4 c). However, with the further addition of PS microspheres, the SEM images of Co-NC-PS (12:1) showed that the macroporous structure collapsed ( Figure 4 d). Figure 5 (a) and 5(b) are the isothermal adsorption-desorption curves and pore size distribution diagrams of Co-NC, respectively. Figure 5(c) and 5(d) are the isothermal adsorption-desorption curves and pore size distribution diagrams of Co-NC-PS (4:1), respectively. Figure 5 (e) and 5(f) are the isothermal adsorption-desorption curves and pore size distribution diagrams of Co-NC-PS, respectively. Figure 5 (g) and 5 (h) are the isothermal adsorption-desorption curves and pore size distribution diagrams of Co-NC-PS (12:1), respectively. It can be seen that with the addition of polystyrene microspheres, the specific surface areas (SSA) of Co-NC, Co-NC-PS (4:1), Co-NC-PS and Co-NC-PS (12:1) are 33.4 m 2 ·g -1 、102.8m 2 ·g -1 、139.9m 2 ·g -1 and 162.5m 2 ·g -1 Among them, Co-NC-PS has more macropores, and the pore size distribution is concentrated in the range of 40 to 80 nm. These results indicate that the PS microsphere template plays a vital role in the formation of 3DOM structure.
[0224] In order to further detect the crystal state of C and Co, the X-ray diffraction (XRD) patterns of the samples are shown in Figure 6 As shown. The XRD spectrum of NC-PS has only two broad diffraction peaks at 22° and 44°, corresponding to the (002) and (100) planes of graphite carbon, respectively. The XRD spectra of Co-NC, Co-NC-PS and Co(X)-NC-PS samples are highly similar to that of NC-PS samples. The Co element has no corresponding diffraction peak, indicating that there may be no Co-containing crystals ( Figure 7 The XRD pattern of NPs Co-NC-PS also showed two sharp narrow peaks at 44.2° and 51.4°, corresponding to the (111) and (200) planes of metal Co, indicating the presence of cobalt particles.
[0225] The graphitization degree and structural defects of all samples were analyzed by Raman spectroscopy. The intensity ratio of D band to G band (I D / I G ) usually represents the degree of structural defects of carbon-based materials. Figure 8 As shown, the I D / I G are 1.04, 1.04 and 1.05 respectively. This indicates that their defect levels are almost the same. D / I G It is significantly smaller (0.96), which may be due to fewer structural defects caused by low degree of N doping in the absence of melamine.
[0226] Co (1.5) -NC-PS, Co (3) -NC-PS, Co (12) -NC-PS, Co-NC-PS, Co (48) -NC-PS and Co (60) The XPS spectra of -NC-PS showed that the Co contents were 0.13, 0.17, 0.25, 0.35, 0.50 and 0.56%, respectively. (1.5) -NC-PS to Co-NC-PS, the enhancement of activity is due to the increase of more metal loading introduced into the Co-N4 active sites. However, with the further addition of metal precursors, the excess metal may be more likely to aggregate into large-sized metal particles. To prove this possibility, we further involved Co (X) -Co 2p XPS spectrum of NC-PS ( Fig. 9 ). (1.5) -NC-PS, Co (3) -NC-PS, Co (12) No Co 2p XPS spectra were detected for either Co-NC-PS or Co-NC-PS. 0 The peak of Co at 778.5 eV indicates that Co exists in a dispersed oxidation state. However, as the amount of Co precursor increases, a Co 0 Corresponding to the acromion, and gradually strengthened. Fig.10 (a) and Fig.10 (b) is Co (48) -TEM image of NC-PS, Fig.10 (c) and Fig.10 (d) is Co (60) -NC-PS TEM image, the presence of large-sized Co particles can be observed, showing that the particle nanoparticles are uniformly embedded in the carbon skeleton. The clear lattice fringes with a spacing of 0.205nm all correspond to the cubic phase Co (111) plane. In summary, the appropriate increase of Co precursor can increase the Co-N4 site and improve the catalytic efficiency. However, excessive Co precursor will lead to the formation of Co particles.
[0227] Although the embodiments of the present invention are disclosed for illustrative purposes, those skilled in the art will appreciate that various substitutions, changes and modifications are possible without departing from the spirit and scope of the present invention and the appended claims. Therefore, the scope of the present invention is not limited to the contents disclosed in the embodiments.
Claims
1. A method for preparing a catalyst for degrading organic pollutants in wastewater, characterized in that: The steps include: Adding chitosan to the first wastewater to obtain floccules, mixing the floccules, transition metal salts, nitrogen sources and pore-forming agents uniformly and freeze-drying the mixture to obtain a precursor, and calcining the precursor at 700-900° C. under the protection of an inert gas to obtain the catalyst, i.e., nitrogen-doped porous carbon supported by a single cobalt atom; Wherein, the first wastewater is wastewater including at least one dye organic pollutant, and the pore-forming agent is polystyrene microspheres; The catalyst includes pores with pore sizes of 40-80 nm and 160-200 nm; The organic pollutant is selected from at least one of methyl orange, azo ruby red, new carmine, orange II and Coomassie brilliant blue; The transition metal salt is selected from at least one of cobalt chloride hexahydrate and cobalt nitrate hexahydrate; The nitrogen source is selected from melamine; The weight ratio of the chitosan to the organic pollutant is 4-6:1; The weight ratio of the flocculant to the transition metal salt is 4.2-62.5:1; The weight ratio of the pore former to the flocculant is 6-12:1; The weight ratio of the transition metal salt to the nitrogen source is 0.05-0.4:1; The specific preparation steps of the precursor are as follows: The flocculants are added to an acid solution, and after being fully dissolved, a transition metal salt and a nitrogen source are added, and after stirring for at least 8 hours, a pore-forming agent is added, and after stirring for at least 8 hours, freeze-dried to obtain a precursor; The specific preparation steps of the catalyst are as follows: The precursor is calcined at 700-900° C. for 1.5-2.5 h, and then naturally cooled to room temperature to obtain the catalyst; wherein the heating rate is 1.5-2.5° C. / min; The acid solution is glacial acetic acid.
2. The preparation method according to claim 1, characterized in that: The precursor is calcined at 800° C. for 2 hours and then naturally cooled to room temperature to obtain the catalyst; wherein the heating rate is 2° C. / min.
3. The preparation method according to claim 1, characterized in that: The weight ratio of the flocculants to the glacial acetic acid is 0.417:
1.
4. A catalyst obtained by the preparation method according to any one of claims 1 to 3.
5. Use of the catalyst as claimed in claim 4 in degrading organic pollutants in wastewater.
6. A method for degrading organic pollutants in wastewater using the catalyst as claimed in claim 4, characterized in that: The steps include: The catalyst is added to the second wastewater containing organic pollutants, and after being evenly dispersed, peroxymonosulfate is added and stirred; Wherein, the organic pollutant includes at least one of bisphenol A, phenol, rhodamine B, methyl orange and 2,4-dichlorophenol; The weight ratio of the catalyst to the organic pollutant is 0.2-0.8:1; The mass concentration of the peroxymonosulfate in the second wastewater is 200-500 mg / L.
Citation Information
Patent Citations
Low-coordination monatomic cobalt catalyst as well as synthesis method and application thereof
CN115445648A