A modified calcium tripolyphosphate, preparation method and application thereof in producing corrosion-resistant ceramic-based-semi-metal friction linings
By using modified calcium tripolyphosphate in the ceramic-based-semi-metallic friction lining, a dense protective layer of polymerized calcium iron phosphate is formed and converted into polycalcium phosphate at high temperatures, thereby solving the problem of the ceramic-based-semi-metallic friction lining. The problems of high cost, corrosion and poor high-temperature strength have been achieved, while good anti-corrosion and high-temperature bonding properties have been achieved.
Patent Information
- Application Number
- CN202310255884.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-16
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2043-03-16
AI Technical Summary
Ceramic-based-semi-metallic friction linings have problems such as high cost, corrosion, and poor high-temperature strength. The existing technology cannot effectively solve these problems.
Modified calcium tripolyphosphate is used, compounded with stearic acid, sodium phenylacetate and laureth phosphate in a mass ratio of 6:3:1, and added to the ceramic-based semi-metallic friction lining to form a dense polymeric iron phosphate. Calcium protective layer to improve rust prevention performance, and converted into calcium polyphosphate at high temperatures to compensate for the loss of organic binder.
It significantly reduces the cost of the lining, improves the anti-corrosion performance and high-temperature bonding strength, and solves the problems of anti-rust and high-temperature strength of the ceramic-based semi-metal friction lining.
Smart Images

Figure GDA0004979453460000091 
Figure GDA0004979453460000111
Abstract
Description
Technical Field
[0001] The present invention relates to a method for preparing a modified calcium tripolyphosphate for a high-strength, corrosion-resistant ceramic-based semi-metal friction lining, and specifically, to a method for preparing the modified calcium tripolyphosphate which can significantly reduce the amount of organic binder in the lining and can give the lining good corrosion resistance and high strength at high temperatures. Background Art
[0002] Ceramic-based semi-metallic friction lining is a new type of friction lining that has emerged in recent years. It fully combines the advantages of traditional ceramic friction lining and semi-metallic friction lining in terms of low noise, wear resistance and large braking force, and is deeply welcomed by consumers. However, there are still some problems in the use of ceramic-based semi-metallic friction lining. First, due to the addition of metal powder in the lining, the lining is at risk of rust. Once the friction lining is rusted, it will have a significant impact on the stability of the friction coefficient and the occurrence of noise. Secondly, traditional ceramic-based semi-metallic friction linings mainly rely on organic binders to bond the raw materials, and organic binders will decompose or thermally decay when the operating temperature is greater than 400°C. Therefore, it is usually only possible to increase the amount of organic binder when preparing the friction lining to make up for the possible losses, which ultimately leads to high costs and safety hazards.
[0003] CN112855814A discloses a low-noise, rust-proof and adhesion-proof drum brake pad for new energy vehicles and a preparation method thereof, wherein the rust-proof ability of the friction lining is improved by not adding rust-prone powders such as iron and adding calcium hydroxide, and by adding zinc powder, the decomposition of the organic binder is inhibited, and the bonding performance at high temperature is improved, thereby obtaining a brake pad with rust-proof and good connectivity. However, the formula does not contain iron and zinc is added, which reduces the strength and increases the cost on the one hand, and on the other hand, the inhibitory effect of zinc powder does not bring the risk of decomposition at higher temperatures.
[0004] CN104315045A discloses a low-cost, low-noise semi-metallic disc brake pad and a preparation method thereof, which improves the bonding performance of the friction lining at high temperature and reduces the cost by adding a silicate ceramic binder. However, since there is no rust-proof treatment in the formula, the friction lining has a certain risk of rust.
[0005] CN101813151A discloses a semi-metal ceramic-based pneumatic disc brake pad and a preparation method thereof, which is pressed and heat-cured according to a conventional dry one-step molding process of resin-based friction materials, and finally machined, ceramicized, inspected and packaged. The semi-metal ceramic-based pneumatic disc brake pad prepared according to the process has large braking torque, comfortable emergency braking, small thermal decay, simple production process, and environmental protection, and is particularly suitable for heavy-duty truck pneumatic disc brakes, but does not consider the amount of rust prevention and organic binder used.
[0006] In summary, the existing ceramic-based semi-metallic friction linings still have problems such as high cost, weak high-temperature bonding strength and rust resistance, so further research is needed. Summary of the invention
[0007] The object of the present invention is to provide a modified calcium tripolyphosphate, a preparation method and its application in the production of high-strength and corrosion-resistant ceramic-based-semi-metallic friction linings, so as to solve the problems of high cost, rust and poor high-temperature strength of the ceramic-based-semi-metallic friction linings mentioned in the above background technology.
[0008] In order to achieve the above technical objectives, the present invention proposes the following solutions:
[0009] A method for preparing modified calcium tripolyphosphate comprises the following steps:
[0010] (1) placing calcium dihydrogen phosphate in a high-temperature furnace under protective gas for calcining to obtain unmodified calcium tripolyphosphate;
[0011] (2) placing the unmodified calcium tripolyphosphate obtained in step (1) in a ball mill, grinding it, and then adding a modifier prepared by mixing stearic acid, sodium phenylacetate and lauryl alcohol ether phosphate to modify it, thereby obtaining a mixed powder;
[0012] (3) The mixed powder obtained by the modification in step (2) is subjected to ultrasonic vibration screening to obtain modified calcium tripolyphosphate.
[0013] Furthermore, the purity of the calcium dihydrogen phosphate described in step (1) is ≥98.0%.
[0014] Furthermore, the protective gas in step (1) is argon.
[0015] Furthermore, the conditions for calcining calcium dihydrogen phosphate in step (1) are: calcining at 350° C. for 6 hours.
[0016] Furthermore, in step (2), the unmodified calcium tripolyphosphate is ground to D100≤15 um.
[0017] Furthermore, the mass ratio of stearic acid, sodium phenylacetate and lauryl ether phosphate in step (2) is 6:3:1.
[0018] The present invention also provides an application of modified calcium tripolyphosphate in the production of high-strength, corrosion-resistant ceramic-based-semi-metal friction linings. The friction linings include the following raw materials: phenolic resin, graphite powder, zinc oxide, silicon carbide, aluminum oxide, refined iron powder, copper powder, modified calcium tripolyphosphate, and DPTT accelerator.
[0019] Furthermore, the friction lining comprises the following raw materials in parts by mass: 20 parts of phenolic resin, 3 parts of graphite powder, 5 parts of zinc oxide, 10 parts of silicon carbide, 10 parts of aluminum oxide, 25 parts of refined iron powder, 5 parts of copper powder, 5 parts of modified calcium tripolyphosphate, and 1 part of DPTT accelerator.
[0020] Furthermore, the preparation method of the friction lining comprises the following steps: putting phenolic resin, graphite powder, zinc oxide, silicon carbide, aluminum oxide, refined iron powder, copper powder, modified calcium tripolyphosphate, and DPTT accelerator into a high-speed mixer and mixing them evenly to obtain a mixture; putting the obtained mixture into a lining mold, pressing at 190°C and 180MPa for 8 minutes to obtain a semi-finished friction lining; putting the obtained semi-finished friction lining into an oven at 180°C and ripening for 15 hours to obtain a high-strength, corrosion-resistant ceramic-based-semi-metallic friction lining.
[0021] The present invention is implemented based on the following principles:
[0022] The present invention intends to add modified calcium tripolyphosphate to the original ceramic-based semi-metal friction lining formula to solve the problems of high cost, rust and poor high temperature strength of the friction lining. The modified calcium tripolyphosphate of the present invention refers to a modifier prepared by compounding stearic acid, sodium phenylacetate and alcohol ether phosphate in a mass ratio of 6:3:1 to solve the compatibility and enhance the anti-rust performance.
[0023] 1. Modified calcium tripolyphosphate mainly improves the anti-rust performance of the system in the following ways
[0024] Since the modified calcium tripolyphosphate has a suitable degree of polymerization of polyphosphate, the polyphosphate can effectively react with Fe 3+ etc. to form a dense polycalcium iron phosphate protective layer, which is adsorbed on the exposed areas to prevent rust.
[0025] 2. Modified calcium tripolyphosphate mainly improves the high temperature adhesion of the system and reduces costs through the following methods
[0026] When the temperature is high, the modified calcium tripolyphosphate will further undergo polymerization reaction, that is, it will generate calcium polyphosphate at high temperature. That is, during use, the organic binder fails at high temperature, and the calcium tripolyphosphate is converted into calcium polyphosphate, which makes up for the loss of the organic resin binder at high temperature, thereby solving the problem of needing to add a large amount of organic resin binder during the preparation process and reducing costs.
[0027] The beneficial effects of the present invention compared with the prior art include:
[0028] The invention is simple and practical. Without making major changes to the original ceramic-based-semi-metal friction material formula and process, the modified calcium tripolyphosphate of the invention is introduced to solve the problems of corrosion resistance, high-temperature adhesion and high cost of the ceramic-based-semi-metal friction lining. The product has a wide range of applications and good market prospects. DETAILED DESCRIPTION
[0029] The advantages of the modified calcium tripolyphosphate of the present invention are specifically reflected in the experimental comparison of the following examples and comparative examples.
[0030] Example 1
[0031] A method for preparing modified calcium tripolyphosphate comprises the following steps:
[0032] 1. Place the purchased calcium dihydrogen phosphate with a purity of ≥98.0% in a high-temperature furnace protected by argon gas and calcine at 350°C for 6 hours to obtain a block intermediate;
[0033] 2. The unmodified intermediate obtained in step 1 is placed in a high-energy ball mill and ground to D100 = 13.521 um, and then a modifier prepared by compounding stearic acid, sodium phenylacetate and lauryl alcohol ether phosphate in a mass ratio of (6:3:1) is added for modification, and the amount of the modifier is 2% of the mass of the unmodified intermediate obtained in step 1;
[0034] 3. The mixed powder obtained by modification in step 2 is sieved by ultrasonic vibration, and the powder obtained by sieving is the modified calcium tripolyphosphate sample described in Example 1.
[0035] Comparative Example 1
[0036] 1. Place the purchased calcium dihydrogen phosphate with a purity of ≥98.0% in a high-temperature furnace protected by argon gas and calcine at 350°C for 3 hours to obtain a block intermediate;
[0037] 2. The unmodified calcium tripolyphosphate obtained in step 1 is placed in a high-energy ball mill and ground to D100 = 13.224 um, and then a modifier prepared by compounding stearic acid, sodium phenylacetate and lauryl alcohol ether phosphate in a mass ratio of (6:3:1) is added for modification, and the amount of the modifier is 2% of the mass of the unmodified intermediate obtained in step 1;
[0038] 3. The mixed powder obtained by the modification in step 2 is sieved by ultrasonic vibration, and the powder obtained by sieving is the sample of comparative example 1.
[0039] Comparative Example 2
[0040] 1. Place the purchased calcium dihydrogen phosphate with a purity of ≥98.0% in a high-temperature furnace protected by argon gas and calcine at 350°C for 6 hours to obtain a block intermediate;
[0041] 2. Place the unmodified calcium tripolyphosphate obtained in step 1 into a high-energy ball mill and grind until D100 = 14.126 um, then stop grinding;
[0042] 3. The mixed powder obtained by the modification in step 2 is sieved by ultrasonic vibration, and the powder obtained by sieving is the sample of comparative example 2.
[0043] Comparative Example 3
[0044] 1. Place the purchased calcium dihydrogen phosphate with a purity of ≥98.0% in a high-temperature furnace protected by argon gas and calcine at 350°C for 6 hours to obtain a block intermediate;
[0045] 2. The unmodified calcium tripolyphosphate obtained in step 1 is placed in a high-energy ball mill and ground to D100 = 12.967 um, and then a modifier prepared by compounding stearic acid, sodium phenylacetate and lauryl alcohol ether phosphate in a mass ratio of (2:5:3) is added for modification, and the amount of the modifier is 2% of the mass of the unmodified intermediate obtained in step 1;
[0046] 3. The mixed powder obtained by the modification in step 2 is sieved by ultrasonic vibration, and the powder obtained by sieving is the sample of comparative example 3.
[0047] Application of modified calcium tripolyphosphate in the production of high-strength, corrosion-resistant ceramic-based semi-metallic friction linings
[0048] Preparation of friction lining No. 1: Take 20 parts by mass of phenolic resin, 3 parts of graphite powder, 5 parts of zinc oxide, 10 parts of silicon carbide, 10 parts of aluminum oxide, 25 parts of refined iron powder, 5 parts of copper powder, 5 parts of sample 1 of Example 1, and 1 part of DPTT accelerator, put them into a high-speed mixer, mix them evenly, and obtain a mixture. Put the mixture into a lining mold, use 190℃, 180MPa, and press for 8min to obtain a semi-finished friction lining. Put the obtained semi-finished friction lining into an oven at 180℃ and mature for 15h to obtain friction lining No. 1.
[0049] Preparation of friction lining No. 2: Take 20 parts by mass of phenolic resin, 3 parts of graphite powder, 5 parts of zinc oxide, 10 parts of silicon carbide, 10 parts of aluminum oxide, 25 parts of refined iron powder, 5 parts of copper powder, 5 parts of sample of comparative example 1, and 1 part of DPTT accelerator, put them into a high-speed mixer, mix them evenly, and obtain a mixture. Put the mixture into a lining mold, use 190℃, 180MPa, press for 8min, and obtain a semi-finished friction lining. Put the obtained semi-finished friction lining into an oven at 180℃ and mature for 15h to obtain friction lining No. 2.
[0050] Preparation of friction lining No. 3: Take 20 parts by mass of phenolic resin, 3 parts of graphite powder, 5 parts of zinc oxide, 10 parts of silicon carbide, 10 parts of aluminum oxide, 25 parts of refined iron powder, 5 parts of copper powder, 5 parts of sample of comparative example 2, and 1 part of DPTT accelerator, put them into a high-speed mixer, mix them evenly, and obtain a mixture. Put the mixture into a lining mold, use 190℃, 180MPa, press for 8min, and obtain a semi-finished friction lining. Put the obtained semi-finished friction lining into an oven at 180℃ and mature for 15h to obtain friction lining No. 3.
[0051] Preparation of friction lining No. 4: Take 20 parts by mass of phenolic resin, 3 parts of graphite powder, 5 parts of zinc oxide, 10 parts of silicon carbide, 10 parts of aluminum oxide, 25 parts of refined iron powder, 5 parts of copper powder, 5 parts of sample of comparative example 3, and 1 part of DPTT accelerator, put them into a high-speed mixer, mix them evenly, and obtain a mixture. Put the mixture into a lining mold, use 190℃, 180MPa, press for 8min, and obtain a semi-finished friction lining. Put the obtained semi-finished friction lining into an oven at 180℃ and mature for 15h to obtain friction lining No. 4.
[0052] Preparation of friction lining No. 5: Put 20 parts by mass of phenolic resin, 3 parts of graphite powder, 5 parts of zinc oxide, 10 parts of silicon carbide, 10 parts of aluminum oxide, 25 parts of refined iron powder, 5 parts of copper powder, and 1 part of DPTT accelerator into a high-speed mixer and mix them evenly to obtain a mixture. Put the mixture into a lining mold and press at 190°C and 180MPa for 8 minutes to obtain a semi-finished friction lining. Put the obtained semi-finished friction lining into an oven at 180°C and mature for 15 hours to obtain friction lining No. 5.
[0053] Various characterization test methods:
[0054] (1) Anti-corrosion performance test
[0055] The friction linings numbered 1-5 prepared as above were tested for friction coefficient according to GB5763-2018, and then several samples were immersed in 5% sodium chloride solution at the same time, and the rust on the appearance was observed. After the rust conditions were obviously different, the friction coefficient was tested again according to the standard.
[0056] (2) High temperature bonding performance test
[0057] Two groups of friction linings numbered 1-5 were prepared. The first group was directly subjected to the impact strength test, and the second group was placed in a 600° C. furnace for 5 minutes and then subjected to the impact strength test.
[0058] Test results:
[0059] (1) Anti-corrosion test results
[0060] The friction linings numbered 1-5 were tested according to the above anti-corrosion performance test method, and the results are shown in Table 1 below:
[0061] Table 1 Anti-corrosion performance test
[0062]
[0063] From the data in Table 1, it can be seen that the corrosion resistance of the friction lining No. 1 is significantly stronger than that of other samples, mainly because:
[0064] 1) For the friction lining No. 2, since the calcination time of the sample of Comparative Example 1 used was too short, the calcium dihydrogen phosphate could not be completely reacted to form calcium tripolyphosphate, and thus the anti-rust effect could not be manifested. Moreover, the friction coefficient of the friction lining No. 1 after immersion was 48.1% higher than that of the friction lining No. 2 after immersion. The friction lining No. 1 had no obvious rust after immersion, while the friction lining No. 2 had a large amount of spotted rust after immersion. It can be seen that the calcium dihydrogen phosphate in step 1 must be placed in a high-temperature furnace protected by argon gas and calcined at 350° C. for a sufficient time, otherwise the friction lining obtained would be difficult to achieve the anti-rust effect.
[0065] 2) For the friction lining No. 3, since the sample of Comparative Example 2 used was not modified with the modifier composed of stearic acid, sodium phenylacetate and lauryl alcohol ether phosphate, calcium tripolyphosphate could not be effectively dispersed in the system, and the anti-corrosion effect was general. The friction coefficient of the friction lining No. 1 after immersion was 29.0% higher than that of the friction lining No. 3 after immersion. The friction lining No. 1 had no obvious rust after immersion, while the friction lining No. 3 had a small amount of spotty rust after immersion. It can be seen that the use of a modifier obtained by compounding stearic acid, sodium phenylacetate and lauryl alcohol ether phosphate to modify calcium tripolyphosphate can greatly improve the anti-rust effect.
[0066] 3) The friction lining No. 4, since the sample of Comparative Example 3 is used, the mass ratio of stearic acid, sodium phenylacetate and lauryl alcohol ether phosphate in the modifier is 2:5:3, and the mass ratio of stearic acid, sodium phenylacetate and alcohol ether phosphate not controlled by the present invention is 6:3:1, and thus the dispersion problem of calcium tripolyphosphate cannot be completely improved, so the anti-rust effect cannot be fully reflected, so that the friction coefficient of the friction lining No. 1 after immersion is 11.1% higher than that of the friction lining No. 4 after immersion. The friction lining No. 1 has no obvious rust after immersion, while the friction lining No. 4 has a small amount of spotty rust after immersion. It can be seen that in order to obtain a good anti-corrosion effect for the friction lining, the formula ratio of the modifier must be strictly controlled.
[0067] 4) The friction lining No. 5. From the data in Table 1, it can be seen that the friction coefficient of the friction lining No. 1 after immersion is 73.9% higher than that of the friction lining No. 5 after immersion. The friction lining No. 1 has no obvious rust after immersion, while the friction lining No. 2 has a large amount of spotted rust after immersion. The reason for this is that the friction lining No. 2 is prepared without adding the modified calcium tripolyphosphate sample of Example 1, so the anti-corrosion effect is extremely poor. It can be seen that adding the modified calcium tripolyphosphate of Example 1 of the present invention in the preparation of the friction lining can significantly improve the friction coefficient of the friction lining after immersion and improve the anti-corrosion effect.
[0068] (2) High temperature bonding performance test results
[0069] The test results according to the above high temperature bonding performance test method are shown in Table 2 below:
[0070] Table 2 High temperature bonding performance test results
[0071]
[0072] From the data in Table 2, it can be seen that the strength of the friction lining No. 1 after high temperature treatment is significantly stronger than that of other samples, mainly because:
[0073] 1) For the friction lining No. 2, since the calcination time of the sample of Comparative Example 1 used was too short, the calcium dihydrogen phosphate could not be completely reacted to form calcium tripolyphosphate, and the time under high temperature treatment was relatively short, the calcium dihydrogen phosphate could not be directly converted into calcium polyphosphate, and the heat loss of the organic binder could not be compensated, so that the impact strength of the friction lining No. 1 after high temperature treatment was 65.0% higher than that of the friction lining No. 2 after high temperature treatment. It can be seen that the calcination of calcium dihydrogen phosphate must be controlled for a sufficient time, otherwise it is difficult for the obtained friction lining to achieve excellent impact strength.
[0074] 2) For the friction lining No. 3, since the sample of Comparative Example 2 used was not modified, calcium tripolyphosphate could not be effectively dispersed in the system to all parts of the lining, resulting in failure to effectively compensate for the loss of the organic binder. As a result, the impact strength of the friction lining No. 1 after high temperature treatment was 24.9% higher than that of the friction lining No. 3 after high temperature treatment. After calcium tripolyphosphate modification, the impact strength of the friction lining can be significantly improved.
[0075] 3) The friction lining No. 4 uses the comparative example 3. Since the mass ratio of stearic acid, sodium phenylacetate and lauryl alcohol ether phosphate in the modifier is 2:5:3, and the mass ratio of stearic acid, sodium phenylacetate and alcohol ether phosphate not controlled by the present invention is 6:3:1, the dispersion problem of calcium tripolyphosphate cannot be completely improved, and thus the heat loss of the organic binder cannot be fully compensated. The impact strength of the friction lining No. 1 after high temperature treatment is 9.6% higher than that of the friction lining No. 4 after high temperature treatment. It can be seen that in order to obtain a higher strength of the friction lining after high temperature treatment, the modifier formula ratio must be controlled.
[0076] 4) For the friction lining No. 5, since no excessive amount of organic resin and the sample of Example 1 were added, the strength of the friction lining after high temperature treatment decreased significantly. Therefore, adding the modified calcium tripolyphosphate of Example 1 of the present invention during the preparation of the friction lining can significantly improve the impact strength of the friction lining after high temperature treatment.
[0077] The above contents are further detailed descriptions of the present invention in combination with specific / preferred implementations, and it cannot be determined that the specific implementation of the present invention is limited to these descriptions. For ordinary technicians in the technical field to which the present invention belongs, they can also make several substitutions or modifications to these described embodiments without departing from the concept of the present invention, and these substitutions or modifications should be regarded as belonging to the protection scope of the present invention.
Claims
1. A method for preparing modified calcium tripolyphosphate, characterized in that: The following steps are involved: (1) placing calcium dihydrogen phosphate in a high-temperature furnace with protective gas and calcining at 350° C. for 6 hours to obtain unmodified calcium tripolyphosphate; (2) placing the unmodified calcium tripolyphosphate obtained in step (1) into a ball mill, grinding it, and then adding a modifier prepared by compounding stearic acid, sodium phenylacetate and lauryl alcohol ether phosphate to modify it, thereby obtaining a mixed powder, wherein the mass ratio of stearic acid, sodium phenylacetate and lauryl alcohol ether phosphate is 6:3:1; (3) The mixed powder obtained by the modification in step (2) is subjected to ultrasonic vibration screening to obtain modified calcium tripolyphosphate.
2. The method for preparing modified calcium tripolyphosphate according to claim 1, wherein The purity of the monocalcium phosphate described in step (1) is ≥98.0%.
3. The preparation method of modified calcium tripolyphosphate according to claim 1, characterized in that, The protective gas in step (1) is argon.
4. The preparation method of modified calcium tripolyphosphate according to claim 1, characterized in that, In step (2), the unmodified calcium tripolyphosphate is ground to D100≤15um.
5. A modified calcium tripolyphosphate prepared according to the method according to any one of claims 1 to 4.
6. Use of the modified calcium tripolyphosphate prepared according to the method of claim 1 in the production of high-strength, corrosion-resistant ceramic-based semi-metallic friction linings, characterized in that: The friction lining comprises the following raw materials: phenolic resin, graphite powder, zinc oxide, silicon carbide, aluminum oxide, refined iron powder, copper powder, modified calcium tripolyphosphate and DPTT accelerator.
7. Use of the modified calcium tripolyphosphate according to claim 6 in the production of high-strength, corrosion-resistant ceramic-based semi-metallic friction linings, characterized in that: The friction lining comprises the following raw materials in parts by mass: 20 parts of phenolic resin, 3 parts of graphite powder, 5 parts of zinc oxide, 10 parts of silicon carbide, 10 parts of aluminum oxide, 25 parts of refined iron powder, 5 parts of copper powder, 5 parts of modified calcium tripolyphosphate, and 1 part of DPTT accelerator.
8. Use of the modified calcium tripolyphosphate according to claim 6 or 7 in the production of high-strength, corrosion-resistant ceramic-based semi-metallic friction linings, characterized in that: The preparation method of the friction lining comprises the following steps: putting phenolic resin, graphite powder, zinc oxide, silicon carbide, aluminum oxide, refined iron powder, copper powder, modified calcium tripolyphosphate and DPTT accelerator into a high-speed stirrer and mixing them evenly to obtain a mixture; putting the obtained mixture into a lining mold and pressing it at 190° C. and 180 MPa for 8 minutes to obtain a semi-finished friction lining; putting the obtained semi-finished friction lining into a 180° C. oven and ripening it for 15 hours to obtain a high-strength and corrosion-resistant ceramic-based-semi-metal friction lining.
Citation Information
Patent Citations
Semimetal ceramic matrix air disc brake pad and production method thereof
CN101813151A
Low-cost low-noise semimetal disc type brake pad and preparation method thereof
CN104315045A
Low-noise and anti-rust-adhesion drum brake pad for new energy vehicle and preparation method thereof
CN112855814A
Flame-retarding and antistatic friction liner for elevator and preparation method of flame-retarding and antistatic friction liner
CN106751435A