A road material for preventing ice and snow melting by phase change and a preparation method thereof
By adding microcapsules with different phase change points into pavement materials, we solve the technical blank problem of phase change materials in the temperature range of -5°C to 5°C in the existing technology, and achieve the optimization of the phase change temperature range and the reduction of the difficulty of ice and snow removal. Effect.
Patent Information
- Application Number
- CN202211095856.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-09-08
- Publication Date
- 2024-10-18
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing anti-icing and snow-melting technology of phase-change mixture pavement has no phase-change material technology in the temperature range of -5℃ to 5℃. Moreover, the phase-change point of existing products is about 13℃ and the enthalpy value is only 70J, making it difficult to meet the requirements of lower temperatures. Anti-ice and snowmelt requirements in temperature ranges.
Microcapsules with different phase change points are used to prepare microcapsules from raw materials such as liquid n-alkanes, deionized water, anhydrous ethanol, cetyltrimethylammonium bromide and tetraethyl orthosilicate, combined with SBS-modified Petroleum asphalt and mineral powder on Route 70 adjust the phase change temperature range of the pavement material to form a wider temperature adjustment range to reduce the consolidation strength between ice and snow and the road surface.
The phase change temperature range is optimized to [-18°C ~ 5°C. The heat released by the phase change material reduces the consolidation strength between ice and snow and the road surface, reduces the difficulty of ice and snow removal, and achieves ice and snow removal with lower mechanical energy.
Smart Images

Figure CN116283063B_ABST
Abstract
Description
Technical Field
[0001] The present application belongs to the field of functional materials, and specifically relates to a pavement material utilizing phase change to prevent ice and snow melting and a preparation method thereof. Background Art
[0002] At present, in the phase change mixture road anti-icing and snow-melting technology, there is still a technical gap in the phase change material that can be applied in engineering and has an optimal temperature range of -5℃ to 5℃. The phase change point of the Beijing Qintian DTC road anti-icing and snow-melting phase change material that has formed a product is about 13℃, and the enthalpy value is only about 70J. Further technical research is needed. Summary of the invention
[0003] In order to solve the problems of the prior art, the present application provides a pavement material utilizing phase change to prevent ice and snow melting and a preparation method thereof, and the present application is implemented through the following scheme:
[0004] A pavement material utilizing phase change to prevent ice and snow melting comprises a substrate and microcapsules at different phase change points dispersed in the substrate.
[0005] Preferably, the microcapsules have a phase transition point of -11°C, -10°C, -3.5°C, or 4°C.
[0006] Preferably, the substrate is an asphalt pavement mixture, and the asphalt pavement mixture includes petroleum asphalt.
[0007] More preferably, SBS-modified No. 70 road petroleum asphalt can be used to replace petroleum asphalt.
[0008] Preferably, the microcapsules are prepared using the following raw materials: liquid normal alkane with 12-15 carbon atoms, deionized water, anhydrous ethanol, hexadecyltrimethylammonium bromide, tetraethyl orthosilicate, and ammonia water.
[0009] Preferably, the amount ratio of the alkane, deionized water, anhydrous ethanol, hexadecyltrimethylammonium bromide, tetraethyl orthosilicate, and ammonia water is 1-15g:1-15g:150-250mL:50-150mL:10-15mL:5-20g:5-20mL.
[0010] A method for preparing a pavement material for anti-icing and snow-melting by phase change, wherein the preparation steps of microcapsules are as follows: (1) a core material, deionized water, anhydrous ethanol, and hexadecyltrimethylammonium bromide are uniformly mixed, and then emulsified for 3-10 minutes under stirring to obtain an emulsion; (2) tetraethyl orthosilicate and ammonia water are sequentially added dropwise to the emulsion obtained in step (1) under stirring, and then reacted for 5 hours, and then stirring was stopped and aged to obtain an emulsion; (3) the emulsion was filtered, washed, and dried to obtain a white powder, i.e., a microcapsule phase change composite material.
[0011] Furthermore, the stirring speed of step (1) is 500-1200 r / min, the stirring speed of step (2) is 1200 r / min, and the reaction temperature of step (2) is 50-70°C.
[0012] Furthermore, the core material is liquid normal alkane, and the normal alkane is one or more of n-dodecane to n-pentadecane.
[0013] Furthermore, the core material is n-dodecane, and the phase transition point of the microcapsule is -11°C; the core material is a mixture of dodecane, tridecane and tetradecane, and the mass ratio of dodecane, tridecane and tetradecane is 8:1:1, and the phase transition point of the microcapsule is -10°C; the core material is a mixture of dodecane, tridecane and tetradecane, and the mass ratio of dodecane, tridecane and tetradecane is 2:1:7, and the phase transition point of the microcapsule is -3.5°C; the core material is a mixture of tridecane, tetradecane and pentadecane, and the mass ratio of tridecane, tetradecane and pentadecane is 2:17:1, and the phase transition point of the microcapsule is 4°C.
[0014] Furthermore, the preparation method of the pavement material is as follows: (1) heating SBS-modified No. 70 road petroleum asphalt to 170°C for use; (2) heating cellulose, fiber stabilizer, coarse aggregate and fine aggregate at 190°C for 2-3h to obtain a premix for use; the particle size of each component of the asphalt pavement mixture meets the SMA-13 grade; (3) adding microcapsules and mineral powder to the premix, stirring for 10-15s, and then adding the heated SBS-modified No. 70 road petroleum asphalt, stirring for 35-45s to obtain the pavement material; the mass ratio of the SBS-modified No. 70 road petroleum asphalt, cellulose, fiber stabilizer, coarse aggregate and fine aggregate is 20-30:0.2-0.5:0.2-0.5:40-50:10-20.
[0015] Furthermore, the microcapsules described in step (3) are microcapsules with a phase change point at 4°C and microcapsules with a phase change point at -3.5°C; the mass ratio of the microcapsules with a phase change point at 4°C and the microcapsules with a phase change point at -3.5°C is 5:1; the amount of the mineral powder is 8-12% of the mass of the premix; the amount of the phase change microcapsules is 0.3-0.8% of the total amount of the mineral powder and the premix.
[0016] The principle of preparing microcapsule phase change composite materials in the present application is: liquid normal alkane is used as the core material, deionized water and anhydrous ethanol are used as the mixed solvent, and hexadecyltrimethylammonium bromide acts as a surfactant, which is hydrophilic and can better attract water to encapsulate oil to form a water-in-oil state. After emulsification is completed, tetraethyl orthosilicate is added to react, and tetraethyl orthosilicate is hydrolyzed to form silanol bonds and then dehydrated and condensed to form silicon-oxygen-silicon bonds. The hydrolyzed silicon-oxygen bonds react with tetraethyl orthosilicate to generate silicon dioxide. As the reaction continues, the generated silicon dioxide gradually replaces the deionized water and eventually becomes a silicon dioxide shell, which encapsulates the liquid normal alkane to form a microcapsule phase change composite material. Taking dodecane as an example, the reaction equation is as follows.
[0017] (a)
[0018] (b)
[0019] (c)n(Si-O-Si)→(-Si-O-Si-)n
[0020] Beneficial effects: The present application achieves the purpose of adjusting the phase change temperature range of the pavement material by adding microcapsules with different phase change points into the pavement material; the phase change temperature range is optimized to a wider temperature adjustment range of [-18°C ~ 5°C], forming a pavement temperature control gradient overlap; although the ice and snow have been solidified with the asphalt pavement when the pavement temperature is continuously below 0°C, when the pavement temperature continues to drop to -3.5°C and -10°C, the phase change material releases heat to form a temperature difference at the junction of the pavement and the ice and snow, greatly reducing the consolidation strength between the ice and snow and the pavement, and the ice and snow can be removed from the pavement with lower mechanical energy, reducing the difficulty of ice and snow removal. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0022] Figure 1 This is a scanning electron microscope 10kx image of C12@SiO2-1;
[0023] Figure 2 This is a scanning electron microscope 30kx image of C12@SiO2-1;
[0024] Figure 3 This is a scanning electron microscope 10kx image of C12@SiO2-2;
[0025] Figure 4This is a scanning electron microscope 30kx image of C12@SiO2-2;
[0026] Figure 5 This is a scanning electron microscope 10kx image of C12@SiO2-3;
[0027] Figure 6 This is a scanning electron microscope 30kx image of C12@SiO2-3;
[0028] Figure 7 This is a scanning electron microscope 10kx image of C12@SiO2-4;
[0029] Figure 8 This is a scanning electron microscope 30kx image of C12@SiO2-4;
[0030] Fig. 9 This is the DSC test curve of A1 microcapsules;
[0031] Fig.10 This is the DSC test curve of A2 microcapsules;
[0032] Fig.11 This is the DSC test curve of A3 microcapsules;
[0033] Fig.12 This is the DSC test curve of A4 microcapsules. DETAILED DESCRIPTION
[0034] In order to make the objectives, technical solutions and advantages of the present application clearer, the implementation methods of the present application will be further described in detail below.
[0035] Example 1
[0036] Preparation of microcapsule C12@SiO2-1 sample:
[0037] The microcapsules are prepared by using the following raw materials: liquid normal alkane with carbon atoms of 12-15, deionized water, anhydrous ethanol, hexadecyltrimethylammonium bromide, tetraethyl orthosilicate and ammonia water.
[0038] The preparation steps of the microcapsule are as follows: (1) 8 g of core material, 200 mL of deionized water, 100 mL of anhydrous ethanol, and 7-8 mL of hexadecyltrimethylammonium bromide are mixed evenly, and then emulsified for 3-10 minutes under stirring to obtain an emulsion; (2) 12 g of tetraethyl orthosilicate and 8 ml of ammonia water are added dropwise to the emulsion obtained in step (1) under stirring, and then reacted for 5 hours, stirring was stopped, and an emulsion was obtained after aging; (3) The emulsion was filtered, washed, and dried to obtain a white powder, which is the microcapsule C12@SiO2-1. The core-shell ratio of the microcapsule C12@SiO2-1 is 4:6; the core material is n-dodecane.
[0039] Preparation of microcapsule C12@SiO2-2 sample:
[0040] The core material is 10 g, tetraethyl orthosilicate is 10 g, and the other preparation methods are the same as those of the microcapsule C12@SiO2-1 sample. The core-shell ratio of the obtained microcapsule C12@SiO2-2 is 5:5.
[0041] Preparation of microcapsule C12@SiO2-3 samples:
[0042] The core material is 12 g, tetraethyl orthosilicate is 8 g, and the other preparation methods are the same as those of the microcapsule C12@SiO2-1 sample. The core-shell ratio of the obtained microcapsule C12@SiO2-3 is 6:4.
[0043] Preparation of microcapsule C12@SiO2-4 sample:
[0044] The core material is 14 g, tetraethyl orthosilicate is 6 g, and the other preparation methods are the same as those of the microcapsule C12@SiO2-1 sample. The core-shell ratio of the obtained microcapsule C12@SiO2-4 is 7:3.
[0045] The scanning electron microscope 10kx and 30kx images of C12@SiO2-1, C12@SiO2-2, C12@SiO2-3, and C12@SiO2-4 are shown in Figures 1-8.
[0046] Preparation of microcapsule samples with a phase transition point of -11°C:
[0047] Microcapsule C12@SiO2-2 is the microcapsule with a phase transition point of -11°C, denoted as A1;
[0048] Preparation of microcapsule samples with a phase transition point of -10℃:
[0049] The core material is a mixture of dodecane, tridecane and tetradecane, and the mass ratio of dodecane, tridecane and tetradecane is 8:1:1. The other preparation methods are the same as those of the microcapsule C12@SiO2-2 sample, which is recorded as A2.
[0050] Preparation of microcapsule samples with a phase transition point of -3,5℃:
[0051] The core material is a mixture of dodecane, tridecane and tetradecane, and the mass ratio of dodecane, tridecane and tetradecane is 2:1:7. The other preparation methods are the same as those of the microcapsule C12@SiO2-2 sample, which is recorded as A3.
[0052] Preparation of microcapsule samples with a phase transition point of 4°C:
[0053] The core material is a mixture of tridecane, tetradecane and pentadecane, and the mass ratio of tridecane, tetradecane and pentadecane is 2:17:1. The rest is the same as the preparation of the microcapsule C12@SiO2-2 sample, which is recorded as A4.
[0054] The DSC test curves of the prepared A1, A2, A3, and A4 microcapsules are as follows: Figure 9-12 .
[0055] Preparation of phase change anti-icing and snow-melting pavement material 1:
[0056] A pavement material for anti-icing and snow melting using phase change, comprising a substrate and microcapsules at different phase change points dispersed in the substrate;
[0057] The substrate is an asphalt pavement mixture, and the asphalt pavement mixture includes SBS-modified No. 70 road petroleum asphalt;
[0058] The preparation method is as follows: (1) SBS-modified No. 70 road petroleum asphalt is heated to 170° C. for use; (2) wood cellulose, fiber stabilizer, coarse sand and gravel, and fine sand and gravel are heated at 190° C. for 2-3 hours to obtain a premix for use; the particle size of each component of the asphalt pavement mixture meets the SMA-13 grade; (3) microcapsules and mineral powder are added to the premix, stirred for 10-15 seconds, and then the heated SBS-modified No. 70 road petroleum asphalt is added, and stirred for 35-45 seconds to obtain pavement material 1;
[0059] The stirring speed of step (1) is 600 r / min, the stirring speed of step (2) is 1200 r / min, and the reaction temperature of step (2) is 65°C.
[0060] The particle size of the coarse sandstone is 3-5 mm, and the particle size of the fine sandstone is 0-3 mm;
[0061] The mass ratio of the SBS-modified No. 70 road petroleum asphalt, wood cellulose, fiber stabilizer, coarse sand and gravel, and fine sand and gravel is 25:0.3:0.3:50:20.
[0062] The amount of the mineral powder is 8-12% of the mass of the premix; the amount of the phase-change microcapsules is 0.3-0.8% of the total amount of the mineral powder and the premix.
[0063] The microcapsule described in step (3) is A1;
[0064] The thermal parameters of pavement material 1 are shown in Table 1.
[0065] Example 2
[0066] Preparation of Phase Change Anti-Ice and Snow Melting Pavement Material II:
[0067] The microcapsule described in step (3) is A2, and the rest is the same as in Example 1;
[0068] The thermal parameters of pavement material 2 are shown in Table 1.
[0069] Example 3
[0070] Preparation of phase change anti-icing and snow-melting pavement material three:
[0071] The microcapsule described in step (3) is A3, and the rest is the same as in Example 1;
[0072] The thermal parameters of pavement material 3 are shown in Table 1.
[0073] Example 4
[0074] Preparation of Phase Change Anti-Ice and Snow Melting Pavement Material IV:
[0075] The microcapsule described in step (3) is A4, and the rest is the same as in Example 1;
[0076] The thermal parameters of pavement material 4 are shown in Table 1.
[0077] Example 5
[0078] The microcapsules in step (3) are A3 and A4, the mass ratio of A3 to A4 is 1:5, and the rest is the same as in Example 1;
[0079] The thermal parameters of pavement material 5 are shown in Table 1.
[0080] Table 1 Thermal parameters of composite phase change materials
[0081]
[0082] Depend on Figure 1-8It can be seen that under the magnification of 10kx, the microcapsule phase change composite material of sample C12@SiO2-2 has the best coating effect, basically presenting a smooth spherical shape, and the structure of the microspheres is relatively uniform; compared with the microcapsule phase change composite material of sample C12@SiO2-1, the microcapsule phase change composite material of sample C12@SiO2-1 also has a smooth spherical coating shape, but the small spheres have partial depressions, and the small spheres are of different sizes, some large and some small; compared with the microcapsule phase change composite material of sample C12@SiO2-2, the microcapsule phase change composite material of sample C12@SiO2-3 also presents a smooth spherical shape, and the small spheres are of similar size, but there are more twinning phenomena. Compared with the microcapsule phase change composite material of sample C12@SiO2-4 and sample C12@SiO2-2, the coating effect of the microcapsule phase change composite material of sample C12@SiO2-4 is not ideal. The size difference of microspheres is too large, the distribution is uneven, and the number of successfully coated microspheres is relatively small. The microspheres are mostly damaged and accompanied by many impurities. Under the magnification of 30kx, the depression of sample C12@SiO2-1 is more obvious, and according to the analysis of the depression of microspheres, there is a situation where the coating is not successful. At the same time, there are a small amount of impurities around the microspheres, which may be impurities caused by organic solvents such as unwashed dodecane or leakage of the microsphere core material. Compared with sample C12@SiO2-1, sample C12@SiO2-2 has good coating effects except for the depression and damage of individual microspheres. After the image of sample C12@SiO2-3 is magnified, its twinning phenomenon is more obvious and there are some impurities near the microspheres. When the twinning phenomenon occurs, the core material leaks or the reagents are not cleaned during the washing stage. At a magnification of 30kx, sample C12@SiO2-4 more clearly finds intermittent impurities near the uncoated microspheres, which deepens the speculation that the impurities are leaks of the core material. After observing and analyzing the magnified SEM images, samples C12@SiO2-1, sample C12@SiO2-3, and sample C12@SiO2-4 exposed more problems. Sample C12@SiO2-2 did not change significantly after magnification and was not accompanied by impurities, which further shows that the core-shell ratio of sample C12@SiO2-2 is the optimal ratio for synthesizing microcapsule phase change composite materials.
[0083] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present application should be included in the protection scope of the present application.
Claims
1. A pavement material utilizing phase change to prevent ice and snow melting, characterized in that: The invention comprises a substrate and microcapsules with different phase transition points dispersed in the substrate; the microcapsules are prepared by using the following raw materials: core material, deionized water, anhydrous ethanol, hexadecyltrimethylammonium bromide, tetraethyl orthosilicate, and ammonia water; the amount ratio of the core material, deionized water, anhydrous ethanol, hexadecyltrimethylammonium bromide, tetraethyl orthosilicate, and ammonia water is 1-15g:150-250mL:50-150mL:10-15mL:5-20g:5-20mL.
2. The pavement material for anti-icing and snow-melting by phase change as claimed in claim 1, characterized in that: The microcapsules have phase transition points of -11°C, -10°C, -3.5°C and 4°C.
3. The pavement material for anti-icing and snow melting by phase change as claimed in claim 2, characterized in that: The substrate is an asphalt pavement mixture, and the asphalt pavement mixture includes SBS-modified No. 70 road petroleum asphalt.
4. The method for preparing a pavement material for anti-icing and snow-melting by phase change as claimed in claim 3, characterized in that: The preparation steps of the microcapsules are as follows: (1) the core material, deionized water, anhydrous ethanol and hexadecyltrimethylammonium bromide are mixed uniformly, and then emulsified for 3-10 minutes under stirring to obtain an emulsion; (2) tetraethyl orthosilicate and ammonia water are sequentially added dropwise to the emulsion obtained in step (1) under stirring, and then reacted for 5 hours, and then stirring was stopped and aged to obtain an emulsion; (3) the emulsion was filtered, washed and dried to obtain a white powder, i.e., a microcapsule phase change composite material.
5. The method for preparing a pavement material for anti-icing and snow-melting by phase change as claimed in claim 4, characterized in that: The stirring speed of step (1) is 500-1200 r / min, the stirring speed of step (2) is 1200 r / min, and the reaction temperature of step (2) is 50-70°C.
6. The method for preparing a pavement material for anti-icing and snow-melting by phase change as claimed in claim 5, characterized in that: The core material is liquid normal alkane, and the normal alkane is one or more of normal dodecane to normal pentadecane.
7. The method for preparing a pavement material for anti-icing and snow-melting by phase change according to claim 6, characterized in that: The core material is n-dodecane, and the phase transition point of the microcapsule is -11°C.
8. The method for preparing a pavement material for anti-icing and snow-melting by phase change according to claim 6, characterized in that: The core material is a mixture of dodecane, tridecane and tetradecane, and the mass ratio of dodecane, tridecane and tetradecane is 8:1:
1. The phase transition point of the microcapsule is -10°C.
9. The method for preparing a pavement material for anti-icing and snow-melting by phase change according to claim 6, characterized in that: The core material is a mixture of dodecane, tridecane and tetradecane, and the mass ratio of dodecane, tridecane and tetradecane is 2:1:
7. The phase transition point of the microcapsule is -3.5°C.
10. The method for preparing a pavement material for anti-icing and snow-melting by phase change according to claim 6, characterized in that: The core material is a mixture of tridecane, tetradecane and pentadecane, and the mass ratio of tridecane, tetradecane and pentadecane is 2:17:
1. The phase transition point of the microcapsule is 4°C.
11. A method for preparing a pavement material for anti-icing and snow-melting by phase change according to claim 7, 8, 9 or 10, characterized in that: The preparation method of the pavement material is as follows: (1) heating SBS-modified No. 70 road petroleum asphalt to 170°C for use; (2) heating cellulose, fiber stabilizer, coarse aggregate and fine aggregate at 190°C for 2-3h to obtain a premix for use; the particle size of each component of the asphalt pavement mixture meets the SMA-13 grade; (3) adding microcapsules and mineral powder to the premix, stirring for 10-15s, and then adding the heated SBS-modified No. 70 road petroleum asphalt, stirring for 35-45s to obtain the pavement material; the mass ratio of the SBS-modified No. 70 road petroleum asphalt, cellulose, fiber stabilizer, coarse aggregate and fine aggregate is 20-30:0.2-0.5:0.2-0.5:40-50:10-20.
12. The method for preparing a pavement material for anti-icing and snow-melting by phase change according to claim 11, characterized in that: The microcapsules described in step (3) are microcapsules with a phase change point at 4°C and microcapsules with a phase change point at -3.5°C; the mass ratio of the microcapsules with a phase change point at 4°C and the microcapsules with a phase change point at -3.5°C is 5:1; the amount of the mineral powder is 8-12% of the mass of the premix; the amount of the phase change microcapsules is 0.3-0.8% of the total amount of the mineral powder and the premix.
Citation Information
Patent Citations
Phase-change temperature-regulating cement asphalt composite concrete
CN111484277A