Inorganic artificial stone plate and preparation method thereof
By using dipolymer cement and alkali exciter to treat iron tailings sand, a three-dimensional network polysilicate gel is formed, which solves the problems of low density and poor durability of inorganic artificial stone slabs, and achieves higher density and strength. Improves the durability and production efficiency of the product.
Patent Information
- Application Number
- CN202211672763.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-26
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2042-12-26
AI Technical Summary
When existing inorganic artificial stone slabs are prepared with cement as cementitious material, they are of low density, low strength and poor durability.
The geopolymer cementing materials include blast furnace granulated slag micro powder, metakaolin and silicon powder, and the iron tailings sand is graded through vibration bulk density test, and the blast furnace granulated slag micro powder, metakaolin, silica fume, crack-resistant fiber, water retention agent and The enhancer is mixed, the alkali activates agent is added and stirred to form a three-dimensional network polysilicate gel to increase the density and strength of the plate.
The density and flexural compressive strength of inorganic artificial stone slabs are improved, the product deformation rate and production cost are reduced, the durability is enhanced, the problem of alkali reflux of ground polymers is slowed, and the production efficiency is improved.
Smart Images

Figure CN116283074B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of building materials, in particular to an inorganic artificial stone plate and a preparation method thereof. Background Art
[0002] Inorganic artificial stone panels are sinter-free panels and are low-energy products. Compared with organic artificial stone panels, the cementing materials used in inorganic artificial stone panels are inorganic, and there is no volatilization of organic solvents during the preparation and use process, which is more environmentally friendly. In addition, inorganic artificial stone panels have better UV aging resistance, high temperature resistance, and flame retardancy than organic panels, and can be used indoors and outdoors, with more diverse application scenarios.
[0003] The cementitious materials used in the preparation of traditional inorganic artificial stone slabs are cement and aggregates. First of all, most of the aggregates are high-quality natural calcium stone and quartz stone, which have high preparation costs, and the mining of natural calcium stone and quartz stone will damage the local environment. Secondly, cement needs to go through the "two grinding and one burning" process during the production process. The burning process consumes a lot of energy and emits a lot of carbon dioxide. According to statistics, the national cement production in 2021 was 2.363 billion tons, and the carbon dioxide emissions were 1.129 billion tons.
[0004] As a major industrial producer, my country has a cumulative stockpile of 62 billion tons of industrial solid waste, of which the total annual production of tailings is about 1.272 billion tons. Among the tailings, iron tailings are the largest, about 520 million tons, accounting for 40.9% of the total tailings. Improving the resource utilization rate of iron tailings is of great significance to alleviating the shortage of existing mineral resources, turning waste into treasure, and ensuring the supply of iron resources.
[0005] Existing iron tailings are often discharged as whole tailings and graded tailings. Directly using iron tailings as aggregates instead of natural calcium stone or quartz stone in artificial stone slabs cannot ensure that the aggregates are in the maximum dense packing state, so the density and strength of the prepared slabs are not high. In addition, the main components of iron tailings sand are ore sand and soil. The presence of soil is not conducive to the formation of cement hydration strength. Iron tailings sand also contains a large amount of sulfur, which will corrode ordinary cement. Therefore, the iron tailings sand inorganic artificial stone slab prepared with cement as the cementitious material is not only low in strength, but also poor in durability. Summary of the invention
[0006] The invention provides an inorganic artificial stone plate and a preparation method thereof, so as to solve the technical problems of low density, low strength and poor durability of the inorganic artificial stone plate prepared by using iron tailings sand using cement as a gelling material.
[0007] According to one aspect of the present invention, an inorganic artificial stone plate is provided, comprising the following raw material components in parts by weight: 6.0 to 10.0 parts of geopolymer binder, 0.9 to 2.1 parts of alkali activator, 16.0 to 19.0 parts of iron tailings, 0.01 to 0.45 parts of water reducer, 0.03 to 1.0 parts of pigment, 0.12 to 0.35 parts of anti-cracking fiber, 0.001 to 0.035 parts of water retaining agent, 0.036 to 0.08 parts of reinforcing agent, and 0.3 to 1.5 parts of water; the geopolymer binder comprises blast furnace granulated slag powder, metakaolin and silica fume.
[0008] Furthermore, the geopolymer binder comprises 35-65% by weight of blast furnace granulated slag powder, 30-60% by weight of metakaolin, and 5-15% by weight of silica fume.
[0009] Furthermore, the specific surface area of the blast furnace granulated slag powder is not less than 400m 2 / kg, activity not less than S95; and / or the metakaolin is a dehydrated product of kaolin calcined at 600-900°C, with a particle size of 325-4000 mesh; and / or the specific surface area of the silica fume is not less than 20000m 2 / kg, of which the silicon dioxide content is not less than 92%.
[0010] Furthermore, the alkaline activator is a mixture of sodium silicate and one or more of potassium silicate, sodium hydroxide or potassium hydroxide; the solid content of the alkaline activator is 50-70%.
[0011] Furthermore, the water reducer includes a polycarboxylic acid water reducer, a naphthalene water reducer or an aminosulfonate water reducer; and / or the anti-cracking fiber includes a synthetic fiber or a basalt fiber.
[0012] Furthermore, the water-retaining agent includes one or more of white sugar, sodium citrate, sodium gluconate, sodium hexametaphosphate and polyethylene glycol.
[0013] Furthermore, the reinforcing agent includes redispersible latex powder, styrene-butadiene latex, polyvinyl alcohol, ethylene-vinyl acetate copolymer or vinyl acetate-versatate copolymer.
[0014] According to another aspect of the present invention, there is also provided a method for preparing an inorganic artificial stone plate, comprising the following steps:
[0015] S1. Divide the iron tailings into at least three grades according to different particle size intervals, apply a vibration bulk density test to obtain the weight ratio of each grade of iron tailings, and mix the iron tailings of each grade according to the weight ratio so that the iron tailings can be tightly combined during the vibration compaction process;
[0016] S2, mixing blast furnace granulated slag powder, metakaolin, silica fume, pigment, anti-cracking fiber, water retaining agent and reinforcing agent, adding the mixed iron tailings sand, mixing and mixing to obtain a dry mix;
[0017] S3, mixing the water reducer and water evenly, adding them to the dry mix, stirring and mixing to obtain a premixed geopolymer mixture, mixing the alkali activator into the premixed geopolymer mixture, and quickly stirring and mixing to obtain a geopolymer geopolymer mixture;
[0018] S4, forming, curing and demoulding the geopolymer mixture to obtain an inorganic artificial stone plate.
[0019] Furthermore, the molding in step S4 is vibration compaction molding, the vacuum degree of the vibration compaction molding is 0.9-1 MPa, the vibration frequency is 50-54 Hz, and the static pressure load is above 200 tons.
[0020] Furthermore, the curing in step S4 also includes post-processing, and the post-processing includes thickness determination, grinding, polishing and deep processing.
[0021] The present invention has the following beneficial effects:
[0022] The inorganic artificial stone board provided by the present invention is a green, low-carbon and environmentally friendly building board, in which the cementitious materials and aggregates are 100% industrial solid waste, replacing high-energy consumption products such as cement, natural calcium stone and natural quartz stone. It can not only improve the utilization rate of industrial solid waste and reduce the pollution to the surrounding environment caused by the dumping of industrial solid waste, but also avoid the processing steps of natural calcium stone and natural quartz stone mining and crushing, thereby reducing the production cost of the product.
[0023] The geopolymer binder used in the present invention is blast furnace granulated slag powder, metakaolin, and silica fume materials with volcanic ash activity. Blast furnace granulated slag powder and metakaolin include aluminosilicates. Under the action of an activator, the solid-phase high-energy aluminum oxygen bond (-Al-O-), silicon oxygen bond (-Si-O-) and other covalent bonds in the aluminosilicates are broken by the action of OH- ions, and the aluminosilicate glass dissociates, releasing the following Si and Al monomers into the solution: [SiO4] and [AlO4]. At the same time, in the alkaline activator environment, the alkaline metal ions (Ga2+) in the above two cementitious materials are 2+ Mg 2+[SiO4] and [AlO4] monomers react with alkali metal ions through dehydroxylation polycondensation to form silicates and aluminosilicates with lower polymerization degree (MSH, ASH, MASH, where M is an alkali metal ion). In this process, according to the principle of chemical reaction equilibrium, the dissolution of aluminosilicates in geopolymer gelling materials will be promoted. [SiO4] and [AlO4] share oxygen atoms and polycondense with alkali metal ions to form a three-dimensional network polysilicate gel. This process is also the main process for the strength formation of geopolymer gelling materials.
[0024] Silica ash has the characteristics of large specific surface area, small particle size, and high silicon dioxide content. Under the action of alkaline activators, the silicon dioxide therein will dissolve and transfer from the solid phase to the liquid phase. At the same time, the high-polymer siliceous components transfer to the oligomeric siliceous components. The addition of silica ash can increase the content of the oligomeric siliceous components in the alkaline activator environment. In addition, the small-sized particles in silica ash are mainly micro-glass spheres, which play a lubricating role on the prepared mixture and facilitate the pressing of the board. Since the micro-glass spheres of silica ash can fill the micropores in the polymer, the flexural and compressive strength of the gelling material is inversely proportional to the porosity, so the addition of silica ash can play a role in improving the strength of the geopolymer gelling material. The geopolymer gelling material used in the present invention is light gray and white, and can be prepared into boards of various colors.
[0025] After the geopolymer is fully in contact with the soil in the iron tailings, the inorganic gel formed by the condensation of the dissolved oligomeric substances will not only wrap around the surface of the soil particles to form inclusions, but also fill the excess gaps between the soil particles, thus forming an interconnected structural system, which can reduce the impact of the soil on strength on a macro scale. In addition, the surface of the soil particles carries Na + or K + , they can carry out equivalent adsorption and exchange with Al in the hydration products of geopolymers, so that smaller soil particles can continuously adsorb and exchange to form large soil aggregates and form strength. Compared with cement, geopolymers can not only play the filling and wrapping role that cement can play, but also react with active substances in the interface of soil particles to form a new inorganic high-density gel system. Geopolymers are synthesized by alkali excitation to form aluminosilicate polymers with a three-dimensional network structure. They have the structural and performance characteristics of high-density materials and inorganic silicate minerals. Compared with traditional silicate cement, they have higher density and corrosion resistance, can reduce the impact of sulfur in iron tailings, and improve the durability of prepared boards.
[0026] The aggregate used in the present invention is iron tailings sand. The preparation method of the inorganic artificial stone plate provided by the present invention obtains iron tailings aggregates of different particle size ranges, and then applies the vibration packing density maximization theory to obtain the optimal ratio of different aggregates, further making the aggregates closely combined during the vibration compaction process, and can complete the pressing 10 to 50 seconds earlier than the original iron tailings sand during the plate forming process, and can also reduce the amount of cementitious materials and reduce the cost of plate production. The prepared plate has a greater density and flexural and compressive strength. The improvement of flexural and compressive strength can reduce the deformation rate of the product and improve the product yield. The increase in density can slow down the problem of geopolymer alkali return. The high density indicates that the prepared plate has a smaller porosity, so it can slow down the precipitation of salt in the geopolymer material, thereby slowing down the undesirable problem of geopolymer alkali return. In addition, shortening the pressing time during the product forming process can improve the production efficiency of the product.
[0027] Aggregates are compacted by vibration in the state of maximum dense packing, which promotes the bite between aggregates and reduces the porosity of aggregates in the stacking state, thereby reducing the amount of cementitious materials used. In addition, geopolymer cementitious materials play a good lubricating role on aggregates during the vibration compaction process of aggregates, promoting the bite or embedding between aggregates. Since geopolymer cementitious materials have a smaller particle size than aggregates, they can fill the pores that cannot be filled by aggregates. They can not only reduce the porosity of the board and increase the overall density of the board, but also play a bonding role on the aggregates after bite. Therefore, the board prepared with geopolymer cementitious materials under this process condition has greater density and strength.
[0028] In addition to the above-described purposes, features and advantages, the present invention has other purposes, features and advantages. The present invention will be further described in detail with reference to the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] The drawings constituting a part of this application are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:
[0030] Figure 1 is a flow chart of the preparation process of a preferred embodiment of the present invention;
[0031] Figure 2 is a vibration packing density diagram of coarse and medium aggregates in different proportions according to Example 1 of the present invention;
[0032] Figure 3 1 is a vibration packing density diagram of coarse and medium aggregates mixed with fine aggregates in different proportions according to Example 1 of the present invention. DETAILED DESCRIPTION
[0033] In order to make the invention purpose, technical scheme and beneficial technical effect of the present invention clearer, the present invention is further described in detail below in conjunction with embodiments. It should be understood that the embodiments described in this specification are only for explaining the present invention, not for limiting the present invention.
[0034] For simplicity, only some numerical ranges are explicitly disclosed herein. However, any lower limit can be combined with any upper limit to form an unambiguous range; and any lower limit can be combined with other lower limits to form an unambiguous range, and any upper limit can be combined with any other upper limit to form an unambiguous range. In addition, although not explicitly stated, each point or single value between the range endpoints is included in the range. Thus, each point or single value can be combined with any other point or single value as its own lower limit or upper limit or with other lower limits or upper limits to form an unambiguous range.
[0035] In the description of this article, it should be noted that, unless otherwise specified, “above” and “below” are inclusive of the number, and the “multiple” in “one or more” means two or more, and the “multiple” in “one or more” means two or more.
[0036] An embodiment of the first aspect of the present application provides an inorganic artificial stone slab, comprising the following raw material components in parts by weight: 6.0 to 10.0 parts of geopolymer binder, 0.9 to 2.1 parts of alkali activator, 16.0 to 19.0 parts of iron tailings, 0.01 to 0.45 parts of water reducer, 0.03 to 1.0 parts of pigment, 0.12 to 0.35 parts of anti-cracking fiber, 0.001 to 0.035 parts of water retaining agent, 0.036 to 0.08 parts of reinforcing agent, and 0.3 to 1.5 parts of water; the geopolymer binder comprises blast furnace granulated slag powder, metakaolin and silica powder.
[0037] In an embodiment of the present invention, the geopolymer binder comprises 35-65% by weight of granulated blast furnace slag powder, 30-60% by weight of metakaolin, and 5-15% by weight of silica fume.
[0038] In some embodiments, the specific surface area of the blast furnace granulated slag powder is not less than 400m 2 / kg, activity not less than S95; and / or the metakaolin is a dehydrated product of kaolin calcined at 600-900°C, with a particle size of 325-4000 mesh; and / or the specific surface area of the silica fume is not less than 20000m 2 / kg, of which the silicon dioxide content is not less than 92%.
[0039] The geopolymer binder used in the present invention is blast furnace granulated slag powder, metakaolin, and silica fume materials with volcanic ash activity. The blast furnace granulated slag powder and metakaolin include aluminosilicates. Under the action of an activator, the covalent bonds of the solid phase high-energy aluminum oxygen bond (-Al-O-), silicon oxygen bond (-Si-O-) and the like in the aluminosilicates are broken by the action of OH- ions, and the aluminosilicate glass is dissociated, releasing the following Si and Al monomers into the solution: [SiO4] and [AlO4]. At the same time, in the alkaline activator environment, the alkaline metal ions Ga in the two cementitious materials are 2+ Mg 2+ The [SiO4] and [AlO4] monomers react with alkali metal ions through dehydroxylation polycondensation to form silicates and aluminosilicates with lower polymerization degree (MSH, ASH, MASH, where M is an alkali metal ion). In this process, according to the principle of chemical reaction equilibrium, the dissolution of aluminosilicates in geopolymer cementitious materials will be promoted. [SiO4] and [AlO4] condense into a three-dimensional network polysilicate gel by sharing oxygen atoms and reacting with alkali metal ions. This process is also the main process for the formation of strength of geopolymer cementitious materials.
[0040] Silica ash has the characteristics of large specific surface area, small particle size and high silicon dioxide content. Under the action of alkaline activator, the silicon dioxide therein will dissolve and transfer from solid phase to liquid phase. At the same time, the high-polymer siliceous component transfers to the oligomeric siliceous component. The addition of silica ash can increase the content of oligomeric siliceous components in the alkaline activator environment. In addition, the small-sized particles in silica ash are mainly micro-glass spheres, which play a lubricating role on the prepared mixture and facilitate the pressing of the board. At the same time, the micro-glass spheres of silica ash can fill the micropores in the polymer, and the flexural and compressive strength of the gelling material is inversely proportional to the porosity. Therefore, the use of silica ash can play a role in improving the strength of the oligomeric gelling material. The geopolymer gelling material used in the present invention is light gray and white, and can be used to prepare boards of various colors.
[0041] In an embodiment of the present invention, the alkaline activator is a mixture of sodium silicate and one or more of potassium silicate, sodium hydroxide or potassium hydroxide; the solid content of the alkaline activator is 50-70%.
[0042] The alkaline activator is a mixture of sodium silicate and one or more of potassium silicate, sodium hydroxide or potassium hydroxide, in which the molar ratio of SiO2 / Na2O, SiO2 / K2O or SiO2 / (Na2O+K2O) is 0.5-1.2.
[0043] According to the embodiment of the present invention, the main function of using the alkali activator in the geopolymer is to disintegrate and polycondense the glass network structure in the geopolymer gelling material, and finally form a geopolymer structure. The reason why the present invention selects the alkali activator solution with a solid content of 50% to 70% is that the prepared mixture needs to be pressed in a semi-dry state, so a low water-binder ratio is required in the process of preparing the mixture. Under the conditions of the same alkali dosage and the same modulus, the higher the solid content of the alkali activator, the less the weight of the activator needs to be added, and it is more convenient to adjust the mixing state of the mixture by adding water. In addition, the high solid content of the alkali activator will increase its viscosity, which is not conducive to its dispersion in the mixture, and is also not conducive to the wetting of the geopolymer gelling material, because the larger the modulus of the alkali activator solution, the higher the silica content, and the greater the viscosity. Therefore, on the basis of selecting an alkali activator solution with a high solid content, selecting a solution with a low modulus is conducive to reducing the viscosity of the alkali activator.
[0044] In an embodiment of the present invention, the water reducer includes a polycarboxylic acid water reducer, a naphthalene water reducer or an aminosulfonate water reducer; and / or the anti-cracking fiber includes a synthetic fiber or a basalt fiber.
[0045] According to an embodiment of the present invention, the use of a pressing plate method to prepare an inorganic artificial stone slab requires that the mixture be in a semi-dry state, that is, the mixture requires a lower water-cement ratio, and the stirred mixture must also ensure that all aggregates and powders can be uniformly wetted and mixed. Therefore, a water reducer is added to the dry mixture together with water, which can make the geopolymer cementitious material powder evenly dispersed, and at the same time release the moisture wrapped in the polymer cementitious material powder, thereby improving the wettability of water to the mixture.
[0046] According to the embodiments of the present invention, the shrinkage performance of the geopolymer cementitious material itself is greater than that of ordinary cement. The use of fiber anti-cracking fibers can act on the geopolymer cementitious material with non-continuous short fibers as reinforcing materials, and limit the development of micro cracks through the cross-linking effect. In addition, the application of anti-cracking fibers can increase the tensile strength of the inorganic artificial stone board, effectively control the micro cracks of the board caused by plastic shrinkage, shrinkage, temperature changes and other factors, prevent or inhibit the formation and development of cracks, and enhance the waterproof and impact resistance of the board.
[0047] According to the embodiments of the present invention, pigments are mainly used to design patterns and / or change the base color of the inorganic artificial stone plate, so that the prepared inorganic artificial stone plate has better aesthetics.
[0048] In an embodiment of the present invention, the water retaining agent includes one or more of white sugar, sodium citrate, sodium gluconate, sodium hexametaphosphate and polyethylene glycol. The water retaining agent can prevent problems such as excessive water loss during the pressing process, resulting in loose pressing.
[0049] In an embodiment of the present invention, the reinforcing agent includes redispersible latex powder, styrene-butadiene latex, polyvinyl alcohol, ethylene-vinyl acetate copolymer or vinyl acetate-versatate copolymer. The reinforcing agent mainly functions to improve strength, increase toughness and reduce water absorption.
[0050] The second aspect of the present application provides a method for preparing the above-mentioned inorganic artificial stone plate, comprising the following steps:
[0051] S1. Divide the iron tailings into at least three grades according to different particle size intervals, apply a vibration bulk density test to obtain the weight ratio of each grade of iron tailings, and mix the iron tailings of each grade according to the weight ratio so that the iron tailings can be tightly combined during the vibration compaction process;
[0052] S2, mixing blast furnace granulated slag powder, metakaolin, silica fume, pigment, anti-cracking fiber, water retaining agent and reinforcing agent, adding the mixed iron tailings sand, mixing and mixing to obtain a dry mix;
[0053] S3, mixing the water reducer and water evenly, adding them to the dry mix, stirring and mixing to obtain a premixed geopolymer mixture, mixing the alkali activator into the premixed geopolymer mixture, and quickly stirring and mixing to obtain a geopolymer geopolymer mixture;
[0054] S4, forming, curing and demoulding the geopolymer mixture to obtain an inorganic artificial stone plate.
[0055] The iron tailings used in some embodiments of the present invention are whole tailings. The iron tailings are divided into 3 to 4 grades of aggregates with different particle size ranges through processes such as drying and screening. The maximum value of the vibration packing density of two large-size aggregates with different weight portions is first determined to form a synthetic proportioned aggregate, and then smaller-size aggregates are added in different proportions, and so on until the maximum vibration packing density of aggregates of various particle size grades is obtained.
[0056] The test steps for the maximum value of vibration bulk density are as follows: (1) weigh the aggregates according to the weight ratio, and mix the aggregates of each grade by mechanical stirring for 3 to 5 minutes to make the aggregates uniform, and then put the mixed aggregates into a 1L cubic container; (2) place the cubic container containing aggregates on a vibration table, turn on the vibration equipment, and continuously add mixed aggregates to the empty space during the vibration process until it is flush with the container mouth, and the aggregates in the container stop falling within 30 to 60 seconds, and then turn off the vibration equipment; (3) pour the aggregates in the cubic container onto the weighing equipment and weigh them to obtain the vibration bulk density of the aggregate.
[0057] In an embodiment of the present invention, the molding in step S4 is vibration compaction molding, the vacuum degree of the vibration compaction molding is 0.9-1MPa, the vibration frequency is 50-54Hz, and the static pressure load is above 200 tons. The curing in step S4 also includes post-processing, and the post-processing includes thickness determination, grinding, polishing and deep processing.
[0058] According to an embodiment of the present invention, in the vibration packing density maximum value test, the vibration frequency of the equipment is between 50 and 54 Hz, which is close to or the same as the vibration frequency of the plate press. Aggregates are weighed by weight ratio before vibration, and each grade of aggregates is mechanically stirred for 3 to 5 minutes to mix the aggregates evenly. The mixed aggregates are loaded into a 1L cube container, and mixed aggregates are continuously added to the vacated space during the vibration process until it is flush with the container mouth. The aggregates in the container no longer drop within 30 to 60 seconds, and the weight of the aggregates in the container is weighed to obtain the vibration packing density of the set. This makes it easier to simulate the state of vibration packing of aggregates during vibration compaction in the plate press, making the test data more accurate.
[0059] According to an embodiment of the present invention, the vibration packing density maximization theory is applied to obtain the best ratio of different aggregates, which further enables the aggregates to be tightly combined during the vibration compaction process, and the pressing can be completed 10 to 50 seconds earlier than the original iron tailings sand during the plate forming process, and the amount of cementitious materials can be reduced, which reduces the cost of plate production. The prepared plate has a greater density and flexural and compressive strength. The improvement of flexural and compressive strength can reduce the deformation rate of the product and improve the product yield; the increase in density can alleviate the problem of geopolymer alkali return. The high density indicates that the prepared plate has a smaller porosity, so it can slow down the precipitation of salt in the geopolymer material, thereby alleviating the problem of geopolymer alkali return. At the same time, shortening the pressing time during the product forming process can improve the production efficiency of the product.
[0060] Aggregates are compacted by vibration in the state of maximum dense packing to promote the bite between aggregates and reduce the porosity of aggregates in the stacking state, thereby reducing the amount of cementitious materials used. Geopolymer cementitious materials lubricate aggregates during the process of aggregate vibration compaction, promoting the bite or embedding between aggregates. Since geopolymer cementitious materials have a smaller particle size, they can fill the parts that cannot be filled by aggregates. This can not only reduce the porosity of the board and increase the overall density of the board, but also play a bonding role for the aggregates after biting. The whole process can make the pressed board have a higher density and a lower porosity, ensuring that the geopolymer iron tailings sand artificial stone board has a higher flexural and compressive strength. Therefore, the board prepared with geopolymer cementitious materials under this process condition has a higher density and strength.
[0061] In some embodiments, a method for preparing a geopolymer iron tailings sand artificial stone plate comprises the following steps:
[0062] S1: Dry and sieve the iron tailings into 3-4 grades of aggregates with different particle sizes. Mix the two grades of aggregates with the largest particle sizes evenly by mechanical stirring for 3-5 minutes according to different weight ratios. Put the mixed aggregates into a 1L cubic container. During the vibration process, continue to add mixed aggregates to the empty space until the aggregates in the container stop decreasing within 30-60 seconds. Weigh the weight of the aggregates in the container, which is the vibration bulk density of the two grades of aggregates. Develop a bulk density curve, and the inflection point of the curve is the maximum vibration bulk density and weight ratio of the two grades of aggregates. Then, add smaller-sized aggregates on the basis of this ratio and repeat the above process to obtain the gradation ratio of the maximum value of the vibration bulk density of all aggregate gradations.
[0063] S2: granulated blast furnace slag powder, metakaolin, silica fume, pigment, water retaining agent, reinforcing agent and anti-cracking fiber are weighed according to weight and put into a mechanical stirring instrument for stirring for 3 to 5 minutes, and then synthetic graded iron ore tailings with the maximum vibration bulk density are added and stirred for 2 to 3 minutes to obtain a dry mix;
[0064] S3: Weigh water and water reducer by weight and mix them evenly to obtain a mixed solution, pour the mixed solution into the dry mix and stir for 2 to 3 minutes to obtain a premixed geopolymer mixture; weigh the alkali activator and add it to the premixed geopolymer mixture, and stir it quickly for 2 to 2.5 minutes to obtain a geopolymer mixture.
[0065] S4: Spread the geopolymer mixture evenly in the template, and form it by vacuuming and vibrating and compacting it for 2 to 5 minutes. After curing at 40 to 80°C for 6 to 24 hours, demould and obtain the rough board. The rough board is subjected to thickness determination, grinding, polishing and deep processing to obtain the geopolymer iron tailings sand artificial stone board.
[0066] The flow chart of the above preparation method is as follows Figure 1 shown.
[0067] Example
[0068] The following examples more specifically describe the disclosure of the present application, which are intended for illustrative purposes only, as it will be apparent to those skilled in the art that various modifications and variations are possible within the scope of the disclosure of the present application. Unless otherwise stated, all parts, percentages, and ratios reported in the following examples are by weight, and all reagents used in the examples are commercially available or synthesized according to conventional methods and can be used directly without further processing, and the instruments used in the examples are commercially available.
[0069] Example 1
[0070] The iron ore tailings used in the embodiments and comparative examples of the present invention are mainly from a mine in Xiangtan, Hunan. The iron ore tailings are dried and sieved into three grades of aggregates with different particle sizes, namely 6-10 mesh (coarse), 20-40 mesh (medium) and 70-120 mesh (fine). The vibration bulk density curves of the two grades of aggregates of 6-10 mesh and 20-30 mesh are obtained by the maximum vibration density test as shown in FIG. Figure 2 Therefore, the coarse and medium iron tailings are mixed in a ratio of 1:0.9, and the vibration bulk density is 1.7501g / cm 2 .
[0071] The coarse and medium aggregates were mixed at a ratio of 1:0.9 and then tested with fine aggregates in different proportions for vibration packing density. The test results are as follows: Figure 3 As shown, Figure 3 As shown in the figure, with the addition of fine iron tailings, the overall vibration bulk density shows a trend of first increasing and then decreasing. The maximum value of the vibration bulk density of coarse + medium: fine is 1.8005g / cm 3 , the weight ratio is m (粗+中) :m (细) =1:0.4. The maximum vibration bulk density of the third-grade iron tailings obtained by this test method is 1.8005 g / cm 3 , at this time the weight ratio of the third grade aggregate is m (粗) :m (中) :m (细) =53:47:40.
[0072] Comparative Example 1
[0073] The iron tailings in Example 1 were dried without screening and directly tested for their vibration bulk density, which was 1.5621 g / cm 2 .
[0074] Comparative Example 2
[0075] The iron tailings sand in Example 1 was dried, screened and configured into a continuously graded aggregate. The vibration bulk density was tested to be 1.6548 g / cm 2 .
[0076] Example 2
[0077] The aggregates are 18.72 parts of the maximum vibration bulk density iron tailings sand mixture configured in Example 1; the amount of geopolymer cementitious material is 6.28 parts, which includes 60% slag powder, 33% kaolin, and 7% silica fume; the activator is a mixture of sodium silicate and potassium silicate with a modulus of 1.2, a solid content of 55.80%, and an amount of 1.22 parts; 0.59 parts of water, 0.013 parts of water reducer, 0.038 parts of reinforcing agent, 0.003 parts of water retaining agent, 0.13 parts of anti-cracking fiber and 0.63 parts of pigment.
[0078] The preparation method of the geopolymer iron tailings sand artificial stone plate of the present embodiment comprises the following steps:
[0079] S1: Weigh 3.77 parts of blast furnace granulated slag powder, 2.07 parts of metakaolin, 0.44 parts of silica fume, 0.63 parts of pigment, 0.13 parts of anti-cracking fiber, 0.003 parts of water retaining agent, and 0.038 parts of reinforcing agent into a mechanical stirring instrument and stir for 4 minutes to ensure that all components are mixed evenly, then add 18.72 parts of synthetic graded iron ore tailings and stir for 2.5 minutes to obtain a dry mix for use;
[0080] S2: Weigh 0.59 parts of water and 0.013 parts of water reducer by weight, mix them evenly, pour them into the dry mix and stir for 2.5 minutes to obtain a premixed geopolymer mixture;
[0081] S3: Weigh 1.22 parts of the alkali activator, pour it into the premixed geopolymer mixture, and stir it rapidly for 2 minutes to obtain the geopolymer mixture;
[0082] S4: Clean the mold and evenly apply the isolation agent inside the mold, spread the geopolymer mixture evenly in the template, and form it by vacuuming and vibrating and compacting for 2.5 minutes. After curing at 60°C for 8 hours, demould and obtain the rough board. The rough board is subjected to thickness determination, grinding, polishing and deep processing to obtain the geopolymer iron tailings sand artificial stone board.
[0083] Example 3
[0084] The aggregates are 17.8 parts of the maximum vibration bulk density iron tailings sand mixture configured in Example 1; the amount of geopolymer cementitious material is 7.30 parts, which includes 59% slag powder, 35% metakaolin, and 6% silica fume; the activator is a mixed solution of sodium silicate and potassium silicate with a modulus of 1.1, a solid content of 56.44%, and an amount of 1.25 parts; 0.84 parts of water, 0.017 parts of water reducer, 0.051 parts of reinforcing agent, 0.004 parts of water retaining agent, 0.16 parts of anti-cracking fiber and 0.62 parts of pigment.
[0085] The preparation method of the geopolymer iron tailings sand artificial stone plate of this embodiment is the same as that of Example 2, and only the components therein need to be replaced.
[0086] Example 4
[0087] The aggregates are 17.7 parts of the maximum vibration bulk density iron tailings sand mixture configured in Example 1; the amount of geopolymer cementitious material is 7.4 parts, which includes 56% slag powder, 36% metakaolin, and 8% silica fume; the activator is a mixed solution of sodium silicate and potassium silicate with a modulus of 1.0, a solid content of 57.16%, and an amount of 1.17 parts; 0.98 parts of water, 0.19 parts of water reducer, 0.053 parts of reinforcing agent, 0.007 parts of water retaining agent, 0.16 parts of anti-cracking fiber and 0.45 parts of pigment.
[0088] The preparation method of the geopolymer iron tailings sand artificial stone plate of this embodiment is the same as that of Example 2, and only the components therein need to be replaced.
[0089] Example 5
[0090] The aggregates are 16.7 parts of the maximum vibration bulk density iron tailings sand mixture configured in Example 1; the amount of geopolymer cementitious material is 8.5 parts, which includes 58% slag powder, 35% metakaolin, and 7% silica fume; the activator is a mixed solution of sodium silicate and potassium silicate with a modulus of 0.9, a solid content of 57.97%, and an amount of 1.32 parts; 0.98 parts of water, 0.022 parts of water reducer, 0.068 parts of reinforcing agent, 0.017 parts of water retaining agent, 0.22 parts of anti-cracking fiber and 0.59 parts of pigment.
[0091] The preparation method of the geopolymer iron tailings sand artificial stone plate of this embodiment is the same as that of Example 2, and only the components therein need to be replaced.
[0092] Example 6
[0093] The aggregates are 16.4 parts of the maximum vibration bulk density iron tailings sand mixture configured in Example 1; the amount of geopolymer cementitious material is 9.0 parts, which includes 53% slag powder, 40% kaolin, and 7% silica fume; the activator is a mixed solution of sodium silicate and potassium silicate with a modulus of 0.8, a solid content of 58.90%, and an amount of 1.30 parts; 1.08 parts of water, 0.036 parts of water reducer, 0.076 parts of reinforcing agent, 0.027 parts of water retaining agent, 0.25 parts of anti-cracking fiber and 0.54 parts of pigment.
[0094] The preparation method of the geopolymer iron tailings sand artificial stone plate of this embodiment is the same as that of Example 2, and only the components therein need to be replaced.
[0095] Example 7
[0096] The aggregates are 16.1 parts of the maximum vibration bulk density iron tailings sand mixture configured in Example 1; the amount of geopolymer cementitious material is 9.4 parts, which includes 45% slag powder, 46% metakaolin, and 9% silica fume; the activator is a mixed solution of sodium silicate and potassium silicate with a modulus of 0.7, a solid content of 59.97%, and an amount of 1.31 parts; 1.26 parts of water, 0.036 parts of water reducer, 0.075 parts of reinforcing agent, 0.033 parts of water retaining agent, 0.28 parts of anti-cracking fiber and 0.45 parts of pigment.
[0097] The preparation method of the geopolymer iron tailings sand artificial stone plate of this embodiment is the same as that of Example 2, and only the components therein need to be replaced.
[0098] Comparative Example 3
[0099] In this comparative example, only the iron ore tailings in Example 3 are replaced by the iron ore tailings in Comparative Example 1, and the amount of tailings and other components remain unchanged.
[0100] The preparation method of the geopolymer iron tailings sand artificial stone board in this comparative example is the same as that in Example 2, except that only the components therein need to be replaced. In addition, the pressing time during the board pressing process needs to be adjusted to 3 minutes.
[0101] Comparative Example 4
[0102] In this comparative example, only the iron ore tailings in Example 3 are replaced by the iron ore tailings in Comparative Example 2, and the amount of tailings and other components remain unchanged.
[0103] The preparation method of the geopolymer iron tailings sand artificial stone board in this comparative example is the same as that in Example 2, except that only the components therein need to be replaced. In addition, the pressing time during the board pressing process needs to be adjusted to 3 minutes.
[0104] Comparative Example 5
[0105] The aggregates are 17.8 parts of the maximum vibration bulk density iron tailings sand mixture configured in Example 1; the cementitious material is 6.96 parts of PW 52.5 white cement; the water reducer is 0.06 parts of polycarboxylic acid water reducer; the reinforcing agent is 0.050 parts, the water retaining agent is 0.014 parts, the anti-cracking fiber is 0.14 parts, the pigment is 0.70 parts, and the water is 1.11 parts.
[0106] The preparation method of the cement-based iron tailings sand artificial stone board of this comparative example comprises the following steps:
[0107] S1: Weigh 6.96 parts of white cement, 0.70 parts of pigment, 0.14 parts of anti-cracking fiber, 0.014 parts of water retaining agent, and 0.050 parts of reinforcing agent in parts by weight, pour them into a mechanical stirring instrument and stir for 4 minutes to ensure that all components are mixed evenly, then add 17.8 parts of synthetic graded iron ore tailings and stir for 2.5 minutes to obtain a dry mix for use;
[0108] S2: Weigh 1.11 parts of water and 0.06 parts of water reducer by weight, mix them evenly, pour them into the dry mix and stir for 2.5 minutes to obtain a cement-based mixture;
[0109] S3: Clean the mold and evenly apply the isolation agent inside the mold, spread the cement-based mixture evenly in the template, and form it by vacuuming and vibrating and compacting it for 2.5 minutes. After curing at 60°C for 24 hours, demould the rough board to obtain the rough board, and then perform thickness determination, grinding, polishing and deep processing on the rough board to obtain the cement-based iron tailings sand artificial stone board.
[0110] In order to highlight the innovation of the formula of the gelling material and the optimized design of the aggregate ratio in the present invention, the performance tests of the above-mentioned embodiments 2 to 7 and comparative examples 3 to 5 were carried out. The test methods were mainly based on GB / T 35160.2-2017 "Synthetic stone test methods Part 2: Determination of flexural strength", GB / T 35160.3-2017 "Synthetic stone test methods Part 3: Determination of compressive strength", and DB44 / T 1601-2015 "Inorganic artificial stone slabs". The specific test results are shown in Table 1.
[0111] Table 1 Performance test results of Examples 2 to 7 and Comparative Examples 3 to 5
[0112]
[0113] *Note: The reference standard is DB44 / T 1601-2015
[0114] As shown in the test of various properties of Examples 2 to 7 and Comparative Examples 3 to 5 in Table 1, firstly, by conducting a vibration packing density maximization test on iron tailings, the artificial stone slabs (Examples 2 to 7) prepared with geopolymer cementitious materials and various admixtures, all the test indicators of the slabs far exceeded the specification value requirements. Secondly, in Comparative Examples 3 and 4 using unscreened iron tailings and continuously graded tailings prepared after screening, it can be seen that even if the pressing time is extended during the plate pressing process, the density and other indicators of the obtained slabs are lower than those of Examples 2 to 7. This is because, in Comparative Examples 3-4, the aggregates cannot reach the maximum dense packing state during the plate pressing process, and the fluidity of the mixture in a semi-dry state is lower than that of the mixture in a plastic state, resulting in some voids that cannot be fully filled with cementitious materials and aggregates. In addition, with regard to Comparative Example 5, the cementitious material used to prepare the board is cement. Even if the iron tailings sand mix ratio in Example 1 is used, the soil component contained in the tailings sand affects the strength of the cement hydration product, and cannot play a good bonding role on the aggregate after the board is pressed and formed. Therefore, even if the pressed board has a large density, its compression and bending strength are still severely reduced, resulting in its water absorption rate, hardness, linear thermal expansion coefficient and other aspects are not as good as other embodiments and other comparative examples. Comparative Example 5 can also prove that the preparation of inorganic artificial stone by combining iron tailings sand with geopolymer in the present invention has certain innovation.
[0115] Although the present application has been described with reference to preferred embodiments, various modifications may be made thereto and parts thereof may be replaced with equivalents without departing from the scope of the present application. In particular, the various technical features mentioned in the various embodiments may be combined in any manner as long as there is no structural conflict. The present application is not limited to the specific embodiments disclosed herein, but includes all technical solutions falling within the scope of the claims.
Claims
1. An inorganic artificial stone plate, characterized in that: The invention comprises the following raw material components in parts by weight: 6.0-10.0 parts of geopolymer binder, 0.9-2.1 parts of alkali activator, 16.0-19.0 parts of iron tailings, 0.01-0.45 parts of water reducer, 0.03-1.0 parts of pigment, 0.12-0.35 parts of anti-cracking fiber, 0.001-0.035 parts of water retaining agent, 0.036-0.08 parts of reinforcing agent, and 0.3-1.5 parts of water; the geopolymer binder comprises blast furnace granulated slag powder, metakaolin and silica powder; The geopolymer binder comprises 35-65% by weight of blast furnace granulated slag powder, 30-60% of metakaolin, and 5-15% of silica fume; The method for preparing an inorganic artificial stone plate comprises the following steps: S1, the dried iron tailings are divided into at least 3 grades according to different particle size intervals, firstly the maximum value of the vibration bulk density of two large-size aggregates with different weight portions is determined to form a synthetic proportioning aggregate, and then smaller aggregates are added in different proportions, and so on until the maximum vibration bulk density of aggregates of multiple different particle size grades is obtained, and the iron tailings of each grade are mixed according to the weight ratio so that the iron tailings can be tightly engaged during the vibration compaction process; S2, mixing blast furnace granulated slag powder, metakaolin, silica fume, pigment, anti-cracking fiber, water retaining agent and reinforcing agent, adding the mixed iron tailings sand, mixing and mixing to obtain a dry mix; S3, mixing the water reducer and water evenly, adding the mixture to the dry mix, stirring and mixing to obtain a premixed geopolymer mixture, mixing the alkali activator into the premixed geopolymer mixture, and rapidly stirring and mixing to obtain a geopolymer mixture; S4, forming, curing and demoulding the geopolymer mixture to obtain an inorganic artificial stone plate.
2. The inorganic artificial stone plate according to claim 1, characterized in that: The specific surface area of the blast furnace granulated slag powder is not less than 400m 2 / kg, activity not less than S95; and / or The metakaolin is a dehydrated product of kaolin calcined at 600-900°C, and has a particle size of 325-4000 meshes; And / or the specific surface area of the silica ash is not less than 20000m 2 / kg, of which the silicon dioxide content is not less than 92%.
3. The inorganic artificial stone plate according to claim 1, characterized in that: The alkaline activator is a mixture of sodium silicate and one or more of potassium silicate, sodium hydroxide or potassium hydroxide; the solid content of the alkaline activator is 50-70%.
4. The inorganic artificial stone plate according to claim 1, characterized in that: The water reducer includes a polycarboxylic acid water reducer, a naphthalene water reducer or an aminosulfonate water reducer; and / or The anti-cracking fiber comprises synthetic fiber or basalt fiber; and / or The pigment includes one or more of titanium dioxide, lead powder, iron black powder, carbon black powder, copper chrome black, iron oxide red, iron oxide blue, medium chrome yellow and red lead powder.
5. The inorganic artificial stone plate according to claim 1, characterized in that: The water retaining agent includes one or more of white sugar, sodium citrate, sodium gluconate, sodium hexametaphosphate and polyethylene glycol.
6. The inorganic artificial stone plate according to claim 1, characterized in that: The reinforcing agent includes redispersible latex powder, styrene-butadiene latex, polyvinyl alcohol, ethylene-vinyl acetate copolymer or vinyl acetate-versatate vinyl ester copolymer.
7. The inorganic artificial stone plate according to claim 1, characterized in that: The molding in step S4 is vibration compaction molding, the vacuum degree of the vibration compaction molding is 0.9-1 MPa, the vibration frequency is 50-54 Hz, and the static pressure load is above 200 tons.
8. The inorganic artificial stone plate according to claim 1, characterized in that: The curing in step S4 also includes post-processing, which includes thickness determination, grinding, polishing and deep processing.