A preparation method and grouting process of grouting material for preventing water damage in coal seam roof

By combining water-based epoxy resin with POSS, nano-silica, bentonite and other materials to form a high-viscosity grouting material, grouting can be used to grout the roof sandstone water damage in coal mining, solving the problem of traditional grouting materials in the Jurassic Coal in the West It solves the problem of poor governance in resources, achieves efficient water blocking and reinforcement effects, reduces costs and avoids environmental pollution.

CN116285374BActive Publication Date: 2024-10-18BEIJING DADI HI TECH GEOLOGICAL EXPLORATION CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202310197066.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-03
Publication Date
2024-10-18
Estimated Expiration
2043-03-03

AI Technical Summary

Technical Problem

In the process of coal mining, traditional cement slurry grouting materials are not effective in controlling water damage in the roof sandstone of the Jurassic coal resources in the West. Moreover, the filling rate and seepage reduction effect of chemical slurries are low, the price is high, and there are environmental pollution hazards.

Method used

A grouting material preparation method is adopted, by combining water-based epoxy resin with POSS, nano-silica, bentonite, aluminum phosphate and other materials to form a grouting material with high viscosity and good permeability, targeting different types of roofs Targeted grouting is carried out for water damage, and the three-dimensional structure of POSS and the role of bentonite during the curing process of epoxy resin are used to fill micro-cracks and form a gel to achieve the water-blocking effect.

Benefits of technology

It effectively solves the problems of poor injectability and unsatisfactory seepage reduction effect of traditional grouting materials in roof sandstone, improves the physical and mechanical properties and stability of the formation, reduces grouting costs, and achieves long-term water blocking effect , avoiding environmental pollution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116285374B_ABST
    Figure CN116285374B_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing a grouting material for water damage on a coal seam roof, comprising the following steps: (1) preparing POSS; (2) preparing an aqueous epoxy resin emulsion; (3) preparing a grouting material; (31) adding the aqueous epoxy resin emulsion into a reaction vessel, adding POSS, mixing evenly, and then reacting at 55-65° C. for 7-9 hours to obtain an epoxy resin-encapsulated POSS emulsion; (32) placing nano silicon dioxide, bentonite, aluminum zinc phosphate hydrate and water into a reaction vessel, and dispersing to obtain a mixed slurry; (33) adding the mixed slurry into the epoxy resin-encapsulated POSS emulsion for high-speed dispersion and stirring, and adding an aqueous epoxy curing agent thereto for secondary mixing to obtain a grouting material for water damage on a coal seam roof. The invention also discloses a grouting process for the grouting material for water damage on a coal seam roof.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of coal water prevention and control, and in particular to a preparation method and a grouting process of a grouting material for preventing water damage in coal seam roof. Background Art

[0002] In recent years, with the large-scale development and utilization of Jurassic coal resources in western my country, the impact and threat of coal seam roof water hazards have become increasingly apparent.

[0003] Mine mining is affected by the sandstone aquifer in the coal seam roof. A large amount of water is discharged during the mining process of the working face, posing a threat of water disasters and frequent impact mine pressure disasters, which have led to serious delays in mine construction, flooding and damage to mining equipment, and shutdown and reduced production of the working face, causing serious economic losses and safety threats to the mine, and seriously interfering with the normal safe production of the mine.

[0004] At present, the main method of water hazard prevention is to grout the advanced area of ​​the coal seam roof rock layer. The selection of grouting materials and engineering technology is the decisive factor in whether the grouting project can achieve the expected goal. The traditional grouting of the limestone layer of the coal seam floor mainly adopts the method of injecting cement slurry into the limestone layer of the coal seam floor to block the water-conducting channels such as fractures and faults to prevent water inrush from the coal seam floor.

[0005] However, the main threat to the development of Jurassic coal resources in western my country is the roof sandstone aquifer, which not only has developed fissures but also contains microcracks and has a high porosity. Since the cement slurry particles are large and cannot enter the internal pores and microcracks of the sandstone strata, it is impossible to completely close the water channel, and there will still be certain potential threats in the coal mining process. In response to this problem, some people have proposed the use of chemical slurries for treatment, but the existing chemical slurries have problems such as low grouting filling rate and seepage reduction effect, high price and certain potential environmental pollution hazards. Summary of the invention

[0006] Purpose of the invention: The present invention aims to improve the problems existing in the above-mentioned prior art, that is, the present invention discloses a preparation method and grouting process of grouting materials for water damage in coal seam roof. The technical problems to be solved by the present invention are: in the process of developing Jurassic coal resources in western my country, the water treatment effect of roof sandstone is not good, cement slurry grouting has poor injectability and is not applicable, the filling rate and seepage reduction effect of chemical slurry are low, the price is high and there are certain potential environmental pollution hazards.

[0007] Technical solution: A method for preparing a grouting material for coal seam roof water damage, which comprises the following steps, calculated by weight:

[0008] (1) Preparation of POSS

[0009] 40-50 parts of water, 14-18 parts of propanol, 3-4 parts of acetonitrile and 0.8-1.2 parts of tetraethylammonium hydroxide are respectively placed in a reaction container, and mixed to obtain a mixed solution, and then 100-120 parts of 3-aminopropyltriethoxysilane are placed in the mixed solution and stirred to obtain a mixed solution, and then the mixed solution is reacted at 45-55° C. for 18-30 hours while stirring to form a white crystalline precipitate, and the white crystalline precipitate is filtered, taken, cleaned with water, and vacuum dried at 90-110° C. to obtain a white powder, that is, POSS;

[0010] (2) Preparation of water-based epoxy resin emulsion

[0011] (21) placing 50-60 parts of epoxy resin in a reactor, and then adding 10-12 parts of a mixed solvent of ethylene glycol monobutyl ether and anhydrous ethanol, heating to 75-85° C., stirring for 0.5-1 h, and completely dissolving the epoxy resin to obtain a mixed solution;

[0012] (22) cooling the mixed solution obtained in step (21) to 45-55° C., adding 70-80 parts of sodium ethylenediaminesulfonate and 10-12 parts of water thereto, and then reacting at 2-4° C. for 2-4 hours to obtain a reaction solution;

[0013] (23) cooling the reaction solution obtained in step (22) to room temperature, then dropwise adding 70-80 parts of ethylenediamine thereto, reacting for 10-12 hours, adding 50-60 parts of deionized water under high-speed stirring, and removing the solvent by reduced pressure distillation to obtain a water-based epoxy resin emulsion;

[0014] (3) Preparation of grouting materials

[0015] (31), adding 40-50 parts of the aqueous epoxy resin emulsion prepared in step (2) into a reaction vessel, and then adding 60-70 parts of the POSS prepared in step (1), mixing well to obtain a mixed solution, and then reacting the mixed solution at 55-65° C. for 7-9 hours to obtain an epoxy resin-encapsulated POSS emulsion;

[0016] (32) placing 30-40 parts of nano-silicon dioxide, 15-25 parts of bentonite, 40-45 parts of aluminum phosphate, and 40-45 parts of zinc hydrate in a reaction container, adding 70-80 parts of water, and grinding and dispersing in a high-speed disperser to obtain a mixed slurry;

[0017] (33) Add 30-40 parts of the mixed slurry obtained in step (32) to 50-55 parts of the epoxy resin-encapsulated POSS emulsion obtained in step (31) for high-speed dispersion and stirring, then add 5-6 parts of water-based epoxy curing agent for secondary mixing, and mix well to obtain a grouting material.

[0018] Furthermore, in the mixed solvent of ethylene glycol monobutyl ether and anhydrous ethanol in step (2), the volume ratio of ethylene glycol monobutyl ether to anhydrous ethanol is 2:1.

[0019] Furthermore, the viscosity of the mixed slurry in step (32) is controlled to be 20-30 mPa·s at room temperature.

[0020] Furthermore, the viscosity of the grouting material obtained in step (3) at room temperature is 60-70 mPa·s.

[0021] Furthermore, the stirring speed of the high-speed stirring in step (23) is 1000-1500 rpm.

[0022] A grouting process for grouting materials for coal seam roof water damage, the steps are as follows:

[0023] (1) Conduct water pressure test on the open hole section of the well to dredge the grouting pipeline and rock cracks in the hole;

[0024] (2) Determine the leakage volume of the open hole section of the well. If the leakage volume is greater than or equal to 30m 3 / h, it is judged that the target layer has developed fractures, that is, it is a fractured aquifer, and the process goes to step (3); if the leakage is less than 30m 3 / h but greater than or equal to 10m 3 / h, it is judged that the cracks in the target layer are relatively developed, that is, it is an aquifer with both pores and cracks, and the process goes to step (3); if the leakage is less than 10m 3 / h, it is judged that the rock formation cracks near the grouting hole are not obviously developed, that is, it is a porous aquifer, and the process goes to step (4);

[0025] (3) Inject cement slurry into the grouting hole, with the stop pressure being 1.2 times the hydrostatic pressure of the aquifer, and then proceed to step (4);

[0026] (4) Inject any of the above-mentioned grouting materials for treating water damage in the coal seam roof into the grouting hole, and stop the grouting pressure at 1.5 times the hydrostatic pressure.

[0027] The mechanism of action of the present invention:

[0028] When the grouting material is used to fill cracks in the coal seam roof water disaster, the viscosity of the grouting material is about 70mPa·s in about 10 minutes, and the viscosity of the grouting material can reach 345.7mPa·s within 1 hour. This grouting material has good fluidity and injectability in the early stage, and the viscosity of the slurry can rise rapidly in the later stage to achieve a good water blocking effect; and the exothermic reaction is not obvious when the slurry gel solidifies.

[0029] In the actual grouting process, the grouting material for coal seam roof water damage (containing water-based epoxy resin slurry and epoxy resin curing agent) is mixed and injected into the porous sandstone formation. The mixture has good permeability in the porous sandstone and forms a gel after curing for a period of time.

[0030] The mechanism of action of bentonite in emulsion is:

[0031]

[0032] The mechanism of action of aluminum phosphate is:

[0033] Al 3+ +OH - =Al(OH)3↓.

[0034] The grouting material for coal seam roof water damage is a composite system, which solves the problem of epoxy resin brittleness itself: during the curing process, epoxy resin is easily subjected to external loads, and cracks will appear inside the material. When the cracks pass through the water-based epoxy resin slurry, the POSS in the epoxy resin is released. The larger three-dimensional structure of POSS absorbs zinc phosphate hydrate and nano-silicon dioxide particles, quickly filling micro-cracks, so that the material can block the cracks for a long time, achieving a good crack repair effect.

[0035]

[0036] Molecular structure of epoxy resin

[0037]

[0038] Synthesis route of waterborne epoxy resin.

[0039] Beneficial effects: The preparation method and grouting process of a grouting material for preventing water damage in coal seam roof disclosed in the present invention have the following beneficial effects:

[0040] 1. A targeted grouting method is proposed for the roof sandstone water, which divides the sandstone aquifer into fissure aquifer, pore aquifer and pore-fissure aquifer, effectively solving the problems of poor injectability and unsatisfactory seepage reduction effect of traditional cement slurry. The filling rate and seepage reduction effect of using chemical slurry alone are low, and there are certain potential environmental pollution hazards.

[0041] 2. Grouting materials can enhance the bonding force between particles, reduce porosity, improve the physical and mechanical properties of the stratum, and enhance the stability of the stratum, so as to achieve the purpose of water blocking, anti-seepage and reinforcement.

[0042] 3. Different grouting methods are used according to the different degrees of crack development in the target layer to achieve targeted grouting, improve grouting effects and reduce grouting costs. BRIEF DESCRIPTION OF THE DRAWINGS

[0043] Figure 1 The present invention discloses a flow chart of a grouting process for a grouting material for preventing water damage in a coal seam roof. DETAILED DESCRIPTION

[0044] The specific embodiments of the present invention are described in detail below.

[0045] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article. Specific embodiment 1

[0047] A method for preparing a grouting material for preventing water damage in a coal seam roof comprises the following steps, measured in parts by mass:

[0048] (1) Preparation of POSS

[0049] 45 parts of water, 16 parts of propanol, 3.5 parts of acetonitrile and 1 part of tetraethylammonium hydroxide are respectively placed in a reaction container, and mixed to obtain a mixed solution. Then 110 parts of 3-aminopropyltriethoxysilane are placed in the mixed solution and stirred to obtain a mixed solution. Then, the mixed solution is reacted at 50° C. for 24 hours while stirring to form a white crystalline precipitate. The white crystalline precipitate is filtered, taken, cleaned with water, and vacuum dried at 100° C. to obtain a white powder, namely, POSS;

[0050] (2) Preparation of water-based epoxy resin emulsion

[0051] (21) placing 55 parts of epoxy resin in a reactor, and then adding 11 parts of a mixed solvent of ethylene glycol monobutyl ether and anhydrous ethanol, heating to 80° C., and stirring for 0.75 h to completely dissolve the epoxy resin to obtain a mixed solution;

[0052] (22) cooling the mixed solution obtained in step (21) to 50° C., adding 75 parts of sodium ethylenediaminesulfonate and 11 parts of water, and then reacting at 3° C. for 3 h to obtain a reaction solution;

[0053] (23) cooling the reaction solution obtained in step (22) to room temperature, then adding 75 parts of ethylenediamine dropwise thereto, reacting for 11 hours, adding 55 parts of deionized water under high-speed stirring, and removing the solvent by reduced pressure distillation to obtain a water-based epoxy resin emulsion;

[0054] (3) Preparation of grouting materials

[0055] (31), adding 45 parts of the aqueous epoxy resin emulsion prepared in step (2) into a reaction container, and then adding 65 parts of the POSS prepared in step (1), mixing well to obtain a mixed solution, and then reacting the mixed solution at 60° C. for 8 hours to obtain an epoxy resin-encapsulated POSS emulsion;

[0056] (32) placing 35 parts of nano-silicon dioxide, 20 parts of bentonite, 42 parts of aluminum phosphate, and 42 parts of zinc hydrate in a reaction container, adding 75 parts of water, and grinding and dispersing in a high-speed disperser to obtain a mixed slurry;

[0057] (33) Add 35 parts of the mixed slurry obtained in step (32) to 52 parts of the epoxy resin-encapsulated POSS emulsion obtained in step (31) for high-speed dispersion and stirring, and then add 5.5 parts of a water-based epoxy curing agent (a water-based epoxy curing agent purchased directly from the market) for secondary mixing, and mix well to obtain a grouting material.

[0058] Furthermore, in the mixed solvent of ethylene glycol monobutyl ether and anhydrous ethanol in step (2), the volume ratio of ethylene glycol monobutyl ether to anhydrous ethanol is 2:1.

[0059] Furthermore, the viscosity of the mixed slurry in step (32) is controlled at 25 mPa·s at room temperature.

[0060] Furthermore, the viscosity of the grouting material obtained in step (3) at room temperature is 64 mPa·s.

[0061] Furthermore, the stirring speed of the high-speed stirring in step (23) is 1300 rpm.

[0062] A grouting process for grouting materials for coal seam roof water damage, the steps are as follows:

[0063] (1) Conduct water pressure test on the open hole section of the well to dredge the grouting pipeline and rock cracks in the hole;

[0064] (2) Determine the leakage volume of the open hole section of the well. If the leakage volume is greater than or equal to 30m 3 / h (i.e., water is pumped inward at a speed of 500L / min for one hour at a pressure of 0), it is determined that fractures are developed in the target layer, i.e., it is a fractured aquifer, and the process goes to step (3); if the leakage is less than 30m 3 / h but greater than or equal to 10m 3 / h, it is judged that the cracks in the target layer are relatively developed, that is, it is an aquifer with both pores and cracks, and the process goes to step (3); if the leakage is less than 10m 3 / h, it is judged that the rock formation cracks near the grouting hole are not obviously developed, that is, it is a porous aquifer, and the process goes to step (4);

[0065] (3) Inject cement slurry into the grouting hole, with the stop pressure being 1.2 times the hydrostatic pressure of the aquifer, and then proceed to step (4);

[0066] (4) Inject any of the above-mentioned grouting materials for treating water damage in the coal seam roof into the grouting hole, and stop the grouting pressure at 1.5 times the hydrostatic pressure.

[0067] Technical demonstration:

[0068] At present, the selection of grouting materials mainly considers two factors: one is the injectability of the material, and the other is the permeability reduction after the injection of the slurry. Among them, the injectability of the slurry is mainly determined by the permeability of the medium along the layer, the rheological properties of the injected slurry, and the size characteristics of the slurry particles. Traditional cement slurry can be injected into pores or cracks with a radius of 0.2mm, while the pores of sandstone are smaller than this value, resulting in poor injectability of cement slurry and inapplicability. Moreover, the permeability resistance of cement slurry during penetration and diffusion at the diameter change and direction change of the seepage channel is too large, causing the migration speed of cement particles to be lower than the speed of water, resulting in particle aggregation and blockage of the channel, insufficient slurry diffusion radius, and too small effective grouting area, making it impossible to achieve the ideal grouting state.

[0069] The particle size of the grouting material for preventing coal seam roof water damage prepared in this embodiment is measured to be 100-400 nm. Therefore, it is feasible to use the grouting material for preventing coal seam roof water damage prepared in this embodiment as a grouting material in terms of injectability.

[0070] The measuring method is: take a small amount of the grouting material for coal seam roof water damage prepared in this embodiment, dilute it with deionized water by 0.5 times, and take the average value after testing it five times with a Japanese Nano-S90 laser particle size analyzer.

[0071] Considering that the viscosity of the grouting material for coal seam roof water damage is relatively high and the porous sandstone seepage channel is fine, it requires a higher grouting pressure. Therefore, at the technical level, the cement slurry is first injected at 1.2 times the hydrostatic pressure, and then the grouting material for coal seam roof water damage prepared in this embodiment is injected at a greater pressure.

[0072] In terms of permeability reduction, the water absorption rate of the grouting material for coal seam roof water damage can be reduced to less than 1% by adjusting the formula, and the minimum water absorption rate is 0.3% when the test time is 30 minutes. Therefore, the grouting material for coal seam roof water damage prepared in this embodiment is also feasible in terms of permeability reduction. When the grouting material for coal seam roof water damage is injected again under the condition of first injecting cement slurry, all water-conducting channels such as cracks, microcracks and pores in the original stratum are blocked, and the water conductivity of the stratum is reduced in the whole space.

[0073] The measurement method is: drip the grouting material for coal seam roof water damage into the sample tank, take out the sample after it is completely cured, weigh its mass G after drying to constant weight, then put it in an appropriate amount of deionized water until it is completely submerged, take out the sample after 48 hours, gently wipe off the moisture on its surface and weigh its mass B at this time. The water absorption rate W is calculated as: At the same time, this chemical slurry can realize the self-repair function, which can repair the micro-cracks caused by external disturbances such as mining after the grouting project, so that the material can seal the cracks for a longer period of time.

[0074] Economic analysis:

[0075] The invention can effectively solve the casualties and property losses caused by accidents such as water leakage from the coal seam roof caused by poor cement slurry injectability during the grouting of the roof sandstone aquifer during the development of Jurassic coal resources in western my country. Since the cost of grouting materials for coal seam roof water damage is relatively high, when the grouting materials for coal seam roof water damage are injected after the cracks are blocked with cement slurry, the dynamic viscosity of the slurry increases, the flow resistance increases, and the diffusion radius of the grouting materials for coal seam roof water damage will decrease, which can reduce the use of grouting materials for coal seam roof water damage to reduce the cost of grouting. Specific embodiment 2

[0077] A method for preparing a grouting material for preventing water damage in a coal seam roof comprises the following steps, measured in parts by mass:

[0078] (1) Preparation of POSS

[0079] 40 parts of water, 14 parts of propanol, 3 parts of acetonitrile and 0.8 parts of tetraethylammonium hydroxide are respectively placed in a reaction container, and mixed to obtain a mixed solution, and then 100 parts of 3-aminopropyltriethoxysilane are placed in the mixed solution and stirred to obtain a mixed solution, and then the mixed solution is reacted at 45° C. for 30 hours while stirring to form a white crystalline precipitate, and the white crystalline precipitate is filtered, taken, cleaned with water, and vacuum dried at 90° C. to obtain a white powder, that is, POSS;

[0080] (2) Preparation of water-based epoxy resin emulsion

[0081] (21) placing 50 parts of epoxy resin in a reactor, and then adding 10 parts of a mixed solvent of ethylene glycol monobutyl ether and anhydrous ethanol, heating to 75° C., stirring for 1 hour to completely dissolve the epoxy resin to obtain a mixed solution;

[0082] (22) cooling the mixed solution obtained in step (21) to 45° C., adding 70 parts of sodium ethylenediaminesulfonate and 10 parts of water thereto, and then reacting at 2° C. for 4 hours to obtain a reaction solution;

[0083] (23) cooling the reaction solution obtained in step (22) to room temperature, then adding 70 parts of ethylenediamine dropwise thereto, reacting for 12 hours, adding 50 parts of deionized water under high-speed stirring, and removing the solvent by reduced pressure distillation to obtain a water-based epoxy resin emulsion;

[0084] (3) Preparation of grouting materials

[0085] (31), adding 40 parts of the aqueous epoxy resin emulsion prepared in step (2) into a reaction container, and then adding 60 parts of the POSS prepared in step (1), mixing well to obtain a mixed solution, and then reacting the mixed solution at 55° C. for 9 hours to obtain an epoxy resin-encapsulated POSS emulsion;

[0086] (32) placing 30 parts of nano-silicon dioxide, 15 parts of bentonite, 40 parts of aluminum phosphate, and 40 parts of zinc hydrate in a reaction container, adding 70 parts of water, and grinding and dispersing in a high-speed disperser to obtain a mixed slurry;

[0087] (33) Add 30 parts of the mixed slurry obtained in step (32) to 50 parts of the epoxy resin-encapsulated POSS emulsion obtained in step (31) for high-speed dispersion and stirring, then add 5 parts of water-based epoxy curing agent for secondary mixing, and mix well to obtain a grouting material.

[0088] Furthermore, in the mixed solvent of ethylene glycol monobutyl ether and anhydrous ethanol in step (2), the volume ratio of ethylene glycol monobutyl ether to anhydrous ethanol is 2:1.

[0089] Furthermore, the viscosity of the mixed slurry in step (32) is controlled at 20.2 mPa·s at room temperature.

[0090] Furthermore, the viscosity of the grouting material obtained in step (3) at room temperature is 60.2 mPa·s.

[0091] Furthermore, the stirring speed of the high-speed stirring in step (23) is 1000 rpm.

[0092] A grouting process for grouting materials for coal seam roof water damage, the steps are as follows:

[0093] (1) Conduct water pressure test on the open hole section of the well to dredge the grouting pipeline and rock cracks in the hole;

[0094] (2) Determine the leakage volume of the open hole section of the well. If the leakage volume is greater than or equal to 30m 3 / h (i.e., water is pumped inward at a speed of 500L / min for one hour at a pressure of 0), it is determined that fractures are developed in the target layer, i.e., it is a fractured aquifer, and the process goes to step (3); if the leakage is less than 30m 3 / h but greater than or equal to 10m3 / h, it is judged that the cracks in the target layer are relatively developed, that is, it is an aquifer with both pores and cracks, and the process goes to step (3); if the leakage is less than 10m 3 / h, it is judged that the rock formation cracks near the grouting hole are not obviously developed, that is, it is a porous aquifer, and the process goes to step (4);

[0095] (3) Inject cement slurry into the grouting hole, with the stop pressure being 1.2 times the hydrostatic pressure of the aquifer, and then proceed to step (4);

[0096] (4) Inject any of the above-mentioned grouting materials for treating water damage in the coal seam roof into the grouting hole, and stop the grouting pressure at 1.5 times the hydrostatic pressure. Specific embodiment 3

[0098] A method for preparing a grouting material for preventing water damage in a coal seam roof comprises the following steps, measured in parts by mass:

[0099] (1) Preparation of POSS

[0100] 50 parts of water, 18 parts of propanol, 4 parts of acetonitrile and 1.2 parts of tetraethylammonium hydroxide are respectively placed in a reaction container, mixed evenly to obtain a mixed solution, and then 120 parts of 3-aminopropyltriethoxysilane are placed in the mixed solution and stirred evenly to obtain a mixed solution, and then the mixed solution is reacted at 55° C. for 18 hours while stirring to form a white crystalline precipitate, filtered, and the white crystalline precipitate is taken, cleaned with water, and vacuum dried at 110° C. to obtain a white powder, that is, POSS;

[0101] (2) Preparation of water-based epoxy resin emulsion

[0102] (21) placing 60 parts of epoxy resin in a reactor, and then adding 12 parts of a mixed solvent of ethylene glycol monobutyl ether and anhydrous ethanol, heating to 85° C., stirring for 0.5 h, so that the epoxy resin is completely dissolved to obtain a mixed solution;

[0103] (22) cooling the mixed solution obtained in step (21) to 55° C., adding 80 parts of sodium ethylenediaminesulfonate and 12 parts of water thereto, and then reacting at 4° C. for 2 h to obtain a reaction solution;

[0104] (23) cooling the reaction solution obtained in step (22) to room temperature, then adding 80 parts of ethylenediamine dropwise thereto, reacting for 10 hours, adding 60 parts of deionized water under high-speed stirring, and removing the solvent by reduced pressure distillation to obtain a water-based epoxy resin emulsion;

[0105] (3) Preparation of grouting materials

[0106] (31), adding 50 parts of the aqueous epoxy resin emulsion prepared in step (2) into a reaction container, and then adding 70 parts of the POSS prepared in step (1), mixing well to obtain a mixed solution, and then reacting the mixed solution at 65° C. for 7 hours to obtain an epoxy resin-encapsulated POSS emulsion;

[0107] (32) placing 40 parts of nano-silicon dioxide, 25 parts of bentonite, 45 parts of aluminum phosphate, and 45 parts of zinc hydrate in a reaction container, adding 80 parts of water, and grinding and dispersing in a high-speed disperser to obtain a mixed slurry;

[0108] (33) Add 40 parts of the mixed slurry obtained in step (32) to 55 parts of the epoxy resin-encapsulated POSS emulsion obtained in step (31) for high-speed dispersion and stirring, then add 6 parts of water-based epoxy curing agent for secondary mixing, and mix well to obtain a grouting material.

[0109] Furthermore, in the mixed solvent of ethylene glycol monobutyl ether and anhydrous ethanol in step (2), the volume ratio of ethylene glycol monobutyl ether to anhydrous ethanol is 2:1.

[0110] Furthermore, the viscosity of the mixed slurry in step (32) is controlled at 29.8 mPa·s at room temperature.

[0111] Furthermore, the viscosity of the grouting material obtained in step (3) at room temperature is 69.5 mPa·s.

[0112] Furthermore, the stirring speed of the high-speed stirring in step (23) is 1500 rpm.

[0113] A grouting process for grouting materials for coal seam roof water damage, the steps are as follows:

[0114] (1) Conduct water pressure test on the open hole section of the well to dredge the grouting pipeline and rock cracks in the hole;

[0115] (2) Determine the leakage volume of the open hole section of the well. If the leakage volume is greater than or equal to 30m 3 / h (i.e., water is pumped inward at a speed of 500L / min for one hour at a pressure of 0), it is determined that fractures are developed in the target layer, i.e., it is a fractured aquifer, and the process goes to step (3); if the leakage is less than 30m 3 / h but greater than or equal to 10m 3 / h, it is judged that the cracks in the target layer are relatively developed, that is, it is an aquifer with both pores and cracks, and the process goes to step (3); if the leakage is less than 10m 3 / h, it is judged that the rock formation cracks near the grouting hole are not obviously developed, that is, it is a porous aquifer, and the process goes to step (4);

[0116] (3) Inject cement slurry into the grouting hole, with the stop pressure being 1.2 times the hydrostatic pressure of the aquifer, and then proceed to step (4);

[0117] (4) Inject any of the above-mentioned grouting materials for treating water damage in the coal seam roof into the grouting hole, and stop the grouting pressure at 1.5 times the hydrostatic pressure.

[0118] The above describes the embodiments of the present invention in detail. However, the present invention is not limited to the above embodiments, and various changes can be made within the knowledge of ordinary technicians in the relevant technical field without departing from the purpose of the present invention.

Claims

1. A method for preparing a grouting material for coal seam roof water damage, characterized in that: The method comprises the following steps, in parts by mass: (1) Preparation of POSS 40-50 parts of water, 14-18 parts of propanol, 3-4 parts of acetonitrile and 0.8-1.2 parts of tetraethylammonium hydroxide are respectively placed in a reaction container, and mixed to obtain a mixed solution, and then 100-120 parts of 3-aminopropyltriethoxysilane are placed in the mixed solution and stirred to obtain a mixed solution, and then the mixed solution is reacted at 45-55° C. for 18-30 hours while stirring to form a white crystalline precipitate, and the white crystalline precipitate is filtered, taken, cleaned with water, and vacuum dried at 90-110° C. to obtain a white powder, that is, POSS; (2) Preparation of waterborne epoxy resin emulsion (21) placing 50-60 parts of epoxy resin in a reactor, and then adding 10-12 parts of a mixed solvent of ethylene glycol monobutyl ether and anhydrous ethanol, heating to 75-85° C., stirring for 0.5-1 h, and completely dissolving the epoxy resin to obtain a mixed solution; (22) cooling the mixed solution obtained in step (21) to 45-55° C., adding 70-80 parts of sodium ethylenediaminesulfonate and 10-12 parts of water thereto, and then reacting at 2-4° C. for 2-4 hours to obtain a reaction solution; (23) cooling the reaction solution obtained in step (22) to room temperature, then dropwise adding 70-80 parts of ethylenediamine thereto, reacting for 10-12 hours, adding 50-60 parts of deionized water under high-speed stirring, and removing the solvent by reduced pressure distillation to obtain a water-based epoxy resin emulsion; (3) Preparation of grouting materials (31), adding 40-50 parts of the aqueous epoxy resin emulsion prepared in step (2) into a reaction vessel, and then adding 60-70 parts of the POSS prepared in step (1), mixing well to obtain a mixed solution, and then reacting the mixed solution at 55-65° C. for 7-9 hours to obtain an epoxy resin-encapsulated POSS emulsion; (32) placing 30-40 parts of nano-silicon dioxide, 15-25 parts of bentonite, 40-45 parts of aluminum phosphate, and 40-45 parts of zinc hydrate in a reaction container, adding 70-80 parts of water, and grinding and dispersing in a high-speed disperser to obtain a mixed slurry; (33) Add 30-40 parts of the mixed slurry obtained in step (32) to 50-55 parts of the epoxy resin-encapsulated POSS emulsion obtained in step (31) for high-speed dispersion and stirring, then add 5-6 parts of water-based epoxy curing agent for secondary mixing, and mix well to obtain a grouting material.

2. The method for preparing a grouting material for preventing water damage in coal seam roof according to claim 1, characterized in that: In the mixed solvent of ethylene glycol monobutyl ether and anhydrous ethanol in step (2), the volume ratio of ethylene glycol monobutyl ether to anhydrous ethanol is 2:

1.

3. The method for preparing a grouting material for treating water damage in a coal seam roof according to claim 1, characterized in that: The viscosity of the mixed slurry in step (32) is controlled to be 20-30 mPa·s at room temperature.

4. The method for preparing a grouting material for treating coal seam roof water damage according to claim 1, characterized in that: The viscosity of the grouting material obtained in step (3) at room temperature is 60-70 mPa·s.

5. The method for preparing a grouting material for preventing water damage in coal seam roof according to claim 1, characterized in that: The stirring speed of the high-speed stirring in step (23) is 1000-1500 rpm.

6. A grouting process for a grouting material for preventing water damage in a coal seam roof prepared by the preparation method according to any one of claims 1 to 5, characterized in that: Here are the steps: (1) Conduct water pressure test on the open hole section of the well to dredge the grouting pipeline and rock cracks in the hole; (2) Determine the leakage volume of the open hole section of the well. If the leakage volume is greater than or equal to 30m 3 / h, it is judged that the target layer has developed fractures, that is, it is a fractured aquifer, and the process goes to step (3); if the leakage is less than 30m 3 / h but greater than or equal to 10m 3 / h, it is judged that the cracks in the target layer are relatively developed, that is, it is an aquifer with both pores and cracks, and the process goes to step (3); if the leakage is less than 10m 3 / h, it is judged that the rock formation cracks near the grouting hole are not obviously developed, that is, it is a porous aquifer, and the process goes to step (4); (3) Inject cement slurry into the grouting hole, with the stop pressure being 1.2 times the hydrostatic pressure of the aquifer, and then proceed to step (4); (4) Inject the grouting material for preventing coal seam roof water damage prepared by the preparation method according to any one of claims 1 to 5 into the grouting hole, and stop the grouting pressure at 1.5 times the hydrostatic pressure.

Citation Information

Patent Citations

  • Nanosized dendrimeric epoxy resin as a loss circulation material

    US20220325165A1

  • Magnesium phosphate cement-based double-liquid grouting material and preparation method therefor

    WO2022083382A1