A method for preparing graphene-modified copper-based composite material
Through the preparation method of graphene-modified copper-based composite materials, combined with sodium dodecylbenzene sulfonate and Y2O3 powder, using molecular blending deposition and vacuum hot-pressing sintering technology, the mechanical properties and conductive properties of copper-based composite materials have been solved. Insufficiency has been achieved, and the comprehensive performance improvement of high strength and high conductivity has been achieved.
Patent Information
- Application Number
- CN202310387685.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-12
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2043-04-12
AI Technical Summary
Existing copper-based composite materials are insufficient in mechanical properties and high-temperature properties, making it difficult to meet the needs of modern working conditions. At the same time, improving mechanical properties will lead to a decrease in electrical conductivity.
A graphene-modified copper-based composite material preparation method is adopted, through molecular blending deposition, thermal reduction, solid-state reaction ball milling and vacuum hot-pressing sintering technology, combined with sodium dodecylbenzene sulfonate as an anionic surfactant and Y2O3 powder , significantly improve the electrical conductivity and mechanical properties of the material.
It achieves the excellent comprehensive properties of high strength and high conductivity of copper-based materials, with an electrical conductivity of 95.6% and a Vickers hardness of 120.8HV0.1, which significantly improves the uniform dispersion and interface bonding of the material, achieving higher density and uniformity. of ultrafine or even nanostructures.
Smart Images

Figure CN116287850B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of high-strength and high-conductivity copper-based composite materials, and specifically relates to a method for preparing a graphene-modified copper-based composite material. The copper-based composite material prepared by the invention is mainly used as a material for resistance welding electrodes, high-power microwave tubes, integrated circuit lead frames, and the like. Background Art
[0002] Copper and copper alloys have many advantages such as easy processing, excellent electrical and thermal properties, etc., and are widely used in the fields of electronics and aerospace, especially in large-scale applications in the electronic information industry such as resistance welding electrodes, integrated circuit lead frames, electric vacuum devices, and high-power microwave tubes. However, due to its deficiencies in mechanical properties and high-temperature properties, it can no longer meet the development needs of today's working conditions. In order to obtain high-performance copper alloys, a second phase is introduced into the copper matrix to prepare copper-based composite materials. For example, the introduction of carbides (SiC) and oxides (Y2O3, AI2O3, HfO2, etc.) as reinforcing phases can significantly improve the mechanical properties of copper alloys, but also limit their electrical conductivity. Summary of the invention
[0003] In response to the problems raised by the background technology, the present invention studies and designs a method for preparing a graphene-modified copper-based composite material, the purpose of which is to provide a method for preparing a graphene-modified copper-based composite material that can not only significantly improve the mechanical properties of the material but also have excellent electrical conductivity and meet the use requirements.
[0004] The technical solution of the present invention:
[0005] A method for preparing a graphene-modified copper-based composite material comprises the following steps:
[0006] Step 1: Molecular blending deposition
[0007] (1) dissolving graphene powder in a graphene water dispersant containing sodium dodecylbenzene sulfonate, and ultrasonically dispersing for 45-60 minutes;
[0008] (2) adding copper nitrate solution to the above solution and continuing ultrasonic dispersion for 2 h to obtain a suspension;
[0009] (3) drying the suspension obtained in step (2) to obtain a copper-loaded graphene composite powder;
[0010] Step 2: Thermal Reduction
[0011] The copper-graphene composite powder obtained in step 1 is placed in a high-temperature tube furnace and thermally reduced under a hydrogen atmosphere to obtain a Cu-Gr composite powder;
[0012] Step 3: Solid phase reaction ball milling
[0013] The Cu-Gr composite powder and Y2O3 powder prepared in step 2 are placed in a ball mill, and the ball mill is assembled in a vacuum glove box under an argon atmosphere. After the assembly is completed, the ball mill is placed in a planetary ball mill for ball milling at a ball milling speed of 300-350 r / min for 10-12 hours. After the ball milling is completed, the ball mill is taken out and ground to finally obtain a dispersed Cu-Y2O3-Gr composite powder;
[0014] Step 4: Vacuum hot pressing sintering
[0015] (1) The Cu-Y2O3-Gr composite powder obtained in step 3 is loaded into the assembled graphite mold, and then the mold is placed on a tray and placed in a vacuum hot pressing sintering furnace, a temperature measuring thermocouple is inserted, an infrared thermometer is aligned, and a vacuum pumping procedure is started;
[0016] (2) The sintering temperature and pressure process curves were set. The temperature was first raised to 600°C and kept at this temperature for 5 min, then raised to 900°C and kept at this temperature for 5 min, and then cooled to room temperature to obtain the Cu-Y2O3-Gr composite material.
[0017] The graphene powder in step 1 has a purity of 99%, a thickness of 3-10 nm, and a diameter of 7-12 μm, and is purchased from Carbon Xi Technology (Shenzhen) Co., Ltd., wherein the mass fraction of the added graphene powder is ≤1%.
[0018] The sodium dodecylbenzenesulfonate in step 1 has a purity of not less than 90% and is purchased from Sinopharm Chemical Reagent Co., Ltd.
[0019] In the step 1, the purity of copper nitrate and graphene water dispersant are both 100%, the concentration of copper nitrate solution is 3 mol / L, the volume of graphene water dispersant added is equal to the volume of copper nitrate solution added, and the graphene water dispersant is purchased from Chengdu Jiacai Technology Co., Ltd.
[0020] The model of the high-temperature tube furnace for the thermal reduction treatment in step 2 is GSL-1200X. The specific process of thermal reduction is to raise the temperature to 550°C-600°C and keep it for 2 hours, then reduce it to 500°C and cool it with the furnace. The heating rate during the thermal reduction process is 10°C / min, and the cooling rate is 10°C / min.
[0021] In the step three, the assembly of the ball mill is completed in a vacuum glove box to ensure a pure ball milling environment. The vacuum glove box model is ZKX, the planetary ball mill is a QM-QX4 all-round planetary ball mill, and the ball milling process is carried out under the protection of an argon atmosphere. The ball mill and the ball milling medium are both made of cemented carbide, the ball milling speed is 300-350 r / min, the ball milling time is 10-12 hours, and the ball-to-material ratio is 5:1.
[0022] The Y2O3 powder in step 3 has a purity of 99.99% and a particle size of 0.5 μm, and is purchased from Shanghai Eon Chemical Technology Co., Ltd.
[0023] The sintering furnace model for vacuum hot pressing sintering in step 4 is FHP-828, the pre-pressing pressure is 10 MPa, the sintering temperature is 900° C., the sintering time is 5 min, and the final pressure is 50 MPa, wherein the heat preservation at 600° C. for 5 min is to remove the contained gas.
[0024] The heating rate of vacuum hot pressing sintering in step 4 is 100° C. / min, and the cooling rate is 100° C. / min.
[0025] The diameter of the graphite mold in step 4 is 30 mm.
[0026] Beneficial effects of the present invention: Different from the traditional copper-based composite material which improves mechanical properties at the expense of electrical and thermal conductivity, the present invention obtains a graphene copper-based composite material with good dispersion through a molecular blending deposition method. The ideal two-dimensional plane structure of graphene and excellent specific surface area make it have very high adsorption capacity, and sodium dodecylbenzene sulfonate, as anionic surfactant, has conductive effect, so that graphene and copper ion have ion II effect, graphene adsorbs a large amount of copper ions to form load copper graphene composite, significantly improves the uniform dispersion of graphene in copper matrix, and obtains excellent electrical conductivity; and oxide particles are added to copper matrix using solid phase reaction ball milling method, reach the effect of dispersion strengthening, matrix alloying improves the interface combination of graphene and copper in this process, significantly improves the mechanical properties of material; vacuum hot pressing sintering technology has the advantages of fast sintering speed, high processing efficiency, high degree of sample densification, and heating, pressurization while acting on the contact diffusion of powder particles, good vacuum degree can reduce sintering temperature in hot pressing process, suppress crystal growth, and remove gas in pores, improve the degree of densification of material, obtain the copper-based alloy with more uniform grain structure and higher density ultrafine or even nanostructure. In general, the composition design and preparation process of the present invention are adopted to achieve the excellent comprehensive performance of high strength and high conductivity of copper-based materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 SEM morphology of Cu-1wt.% Y2O3-0.3wt.% Gr composite material bulk at 2000 times.
[0028] Figure 2 This is the tensile fracture morphology of Cu-1wt.% Y2O3-0.3wt.% Gr composite material under 3000 times tensile strength.
[0029] Figure 3The metallographic structure diagram of Cu-1wt.%Y2O3-0.3wt.%Gr composite material at 1000 times. DETAILED DESCRIPTION
[0030] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments.
[0031] Example 1
[0032] The Cu-Y2O3-Gr composite material in this embodiment is made by molecular blending deposition, thermal reduction, solid phase reaction ball milling and vacuum hot pressing sintering, wherein the mass fraction of Y2O3 is 1% and the mass fraction of Gr is 0.1%.
[0033] The preparation method of the Cu-Y2O3-Gr composite material in this embodiment is as follows:
[0034] Step 1, molecular blending deposition: first, dissolve 0.02g of graphene powder with a purity of 99% in a graphene water dispersant containing sodium dodecylbenzene sulfonate, the volume of the graphene water dispersant is 103ml, the amount of sodium dodecylbenzene sulfonate added is 0.5g, and ultrasonic dispersion is performed for 45min; add 103ml of 3mol / L copper nitrate solution to the above solution and continue ultrasonic dispersion for 2h to obtain a suspension, dry the obtained suspension to obtain a precursor, and fully grind the obtained precursor in a mortar to obtain a copper-loaded graphene composite powder;
[0035] Step 2, thermal reduction: placing the above-obtained copper-graphene composite powder in a high-temperature tubular furnace, and thermally reducing it in a hydrogen atmosphere to obtain a Cu-Gr composite powder; the thermal reduction temperature is raised to 600°C and kept for 2 hours, then lowered to 500°C and cooled with the furnace, wherein the heating rate is 10°C / min, and the cooling rate is 10°C / min;
[0036] Step 3, solid phase reaction ball milling: The Cu-Gr composite powder and Y2O3 powder prepared in step 2 are placed in a ball mill, the mass fraction of Y2O3 is 1%, and the ball mill is assembled in a vacuum glove box under an argon atmosphere, and the ball milling process is carried out under the protection of an argon atmosphere. The ball mill and the ball milling medium are both made of cemented carbide. After the assembly is completed, the ball mill is placed in a planetary ball mill for ball milling. The ball milling speed is 300 r / min and the ball milling time is 10 hours. After the ball milling is completed, the ball mill is taken out and ground to finally obtain 20 g of dispersed Cu-Y2O3-Gr composite powder;
[0037] Step 4, vacuum hot pressing sintering: The Cu-Y2O3-Gr composite powder obtained in step 3 is loaded into the assembled graphite mold, and then the mold is placed on a tray and placed in a vacuum hot pressing sintering furnace, and a temperature measuring thermocouple is inserted, aligned with the infrared thermometer, and the vacuum program is started; the sintering temperature and pressure process curve are set, first the temperature is raised to 600°C and kept warm for 5 minutes, then the temperature is raised to 900°C and kept warm for 5 minutes, and then the temperature is lowered to room temperature after the insulation is completed to obtain the Cu-Y2O3-Gr composite material.
[0038] Example 2
[0039] The Cu-Y2O3-Gr composite material in this embodiment is made by molecular blending deposition, thermal reduction, solid phase reaction ball milling and vacuum hot pressing sintering, wherein the mass fraction of Y2O3 is 1% and the mass fraction of Gr is 0.3%.
[0040] The preparation method of the Cu-Y2O3-Gr composite material in this embodiment is as follows:
[0041] Step 1, molecular blending deposition: first, dissolve 0.06g of graphene powder with a purity of 99% in a graphene water dispersant containing sodium dodecylbenzene sulfonate, the volume of the graphene water dispersant is 102.8ml, the amount of sodium dodecylbenzene sulfonate added is 0.5g, and ultrasonic dispersion is performed for 55min; add 102.8ml of 3mol / L copper nitrate solution to the above solution and continue ultrasonic dispersion for 2h to obtain a suspension, dry the obtained suspension to obtain a precursor, and fully grind the obtained precursor in a mortar to obtain a copper-loaded graphene composite powder;
[0042] Step 2, thermal reduction: placing the above-obtained copper-graphene composite powder in a high-temperature tubular furnace, thermally reducing it in a hydrogen atmosphere to obtain a Cu-Gr composite powder, the thermal reduction temperature is raised to 600°C and kept for 2 hours, then lowered to 500°C and cooled with the furnace, wherein the heating rate is 10°C / min, and the cooling rate is 10°C / min;
[0043] Step 3, solid phase reaction ball milling: The Cu-Gr composite powder and Y2O3 powder prepared in step 2 are placed in a ball mill, the mass fraction of Y2O3 is 1%, and the ball mill is assembled in a vacuum glove box under an argon atmosphere, and the ball milling process is carried out under the protection of an argon atmosphere. The ball mill and the ball milling medium are both made of cemented carbide. After the assembly is completed, the ball mill is placed in a planetary ball mill for ball milling. The ball milling speed is 325 r / min, and the ball milling time is 11 hours. After the ball milling is completed, the powder is taken out and ground to finally obtain 20 g of dispersed Cu-Y2O3-Gr composite powder;
[0044] Step 4, vacuum hot pressing sintering: The Cu-Y2O3-Gr composite powder obtained in step 3 is loaded into the assembled graphite mold, and then the mold is placed on a tray and placed in a vacuum hot pressing sintering furnace, and a temperature measuring thermocouple is inserted, aligned with the infrared thermometer, and the vacuum program is started; the sintering temperature and pressure process curve are set, first the temperature is raised to 600°C and kept warm for 5 minutes, then the temperature is raised to 900°C and kept warm for 5 minutes, and then the temperature is lowered to room temperature after the insulation is completed to obtain the Cu-Y2O3-Gr composite material.
[0045] Example 3
[0046] The Cu-Y2O3-Gr composite material in this embodiment is made by molecular blending deposition, thermal reduction, solid phase reaction ball milling and vacuum hot pressing sintering, wherein the mass fraction of Y2O3 is 1% and the mass fraction of Gr is 0.5%.
[0047] The preparation method of the Cu-Y2O3-Gr composite material in this embodiment is as follows:
[0048] Step 1, molecular blending deposition: first, dissolve 0.1g of graphene powder with a purity of 99% in a graphene water dispersant containing sodium dodecylbenzene sulfonate, the volume of the graphene water dispersant is 102.6ml, the amount of sodium dodecylbenzene sulfonate added is 0.5g, and ultrasonic dispersion is performed for 60min; add 102.6ml of 3mol / L copper nitrate solution to the above solution and continue ultrasonic dispersion for 2h to obtain a suspension, dry the obtained suspension to obtain a precursor, and then fully grind the obtained precursor in a mortar to obtain a copper-loaded graphene composite powder;
[0049] Step 2, thermal reduction: placing the above-obtained copper-graphene composite powder in a high-temperature tubular furnace, and thermally reducing it in a hydrogen atmosphere to obtain a Cu-Gr composite powder; the thermal reduction temperature is raised to 600°C and kept for 2 hours, then lowered to 500°C and cooled with the furnace, wherein the heating rate is 10°C / min, and the cooling rate is 10°C / min;
[0050] Step 3, solid phase reaction ball milling: The Cu-Gr composite powder and Y2O3 powder prepared in step 2 are placed in a ball mill, the mass fraction of Y2O3 is 1%, and the ball mill is assembled in a vacuum glove box under an argon atmosphere, and the ball milling process is carried out under the protection of an argon atmosphere. The ball mill and the ball milling medium are both made of cemented carbide. After the assembly is completed, the ball mill is placed in a planetary ball mill for ball milling. The ball milling speed is 350 r / min and the ball milling time is 12 hours. After the ball milling is completed, the ball mill is taken out and ground to finally obtain 20 g of dispersed Cu-Y2O3-Gr composite powder;
[0051] Step 4, vacuum hot pressing sintering: The Cu-Y2O3-Gr composite powder obtained in step 3 is loaded into the assembled graphite mold, and then the mold is placed on a tray and placed in a vacuum hot pressing sintering furnace, and a temperature measuring thermocouple is inserted, aligned with the infrared thermometer, and the vacuum program is started; the sintering temperature and pressure process curve are set, first the temperature is raised to 600°C and kept warm for 5 minutes, then the temperature is raised to 900°C and kept warm for 5 minutes, and then the temperature is lowered to room temperature after the insulation is completed to obtain the Cu-Y2O3-Gr composite material.
[0052] The performance of the Cu-Y2O3-Gr composite materials prepared in Examples 1 to 3 was tested, and the test results are shown in Table 1:
[0053] Table 1 Test results of electrical conductivity and Vickers hardness of Cu-Y2O3-Gr composite materials in Examples 1 to 3
[0054] Material Conductivity (%IACS) <![CDATA[Hardness (HV 0.1 )]]> <![CDATA[Cu-1wt.%Y2O3]]> 85.6% 125.6 <![CDATA[Cu-1wt.%Y2O3-0.1wt.%Gr]]> 92.5% 117.3 <![CDATA[Cu-1wt.%Y2O3-0.3wt.%Gr]]> 95.6% 120.8 <![CDATA[Cu-1wt.%Y2O3-0.5wt.%Gr]]> 91.8% 105.2
[0055] Depend on Figure 1 It can be seen that graphene in the Cu-1wt.% Y2O3-0.3wt.% Gr composite material is mainly distributed at the grain boundaries of the copper matrix.
[0056] Depend on Figure 2 It can be seen that the Cu-1wt.% Y2O3-0.3wt.% Gr composite material undergoes ductile fracture under tension. The addition of Gr increases the space for heterogeneous nucleation, and the grain refinement of graphene reduces the stress generated by dislocation pile-up, resulting in dimples or tear edges. Therefore, the fracture surface mainly presents a dimple morphology, and flaky graphene can be observed inside the dimples.
[0057] Depend on Figure 3 It can be seen that the graphene in the Cu-1wt.% Y2O3-0.3wt.% Gr composite material is evenly dispersed on the grain boundaries of the copper matrix. Graphene has a pinning effect on dislocations and grain boundary movement, the grains are significantly refined, and the composition is more uniform, which effectively improves the microstructure of the copper alloy composite material and enhances the mechanical properties of the copper alloy composite material.
[0058] As can be seen from Table 1, compared with the traditional copper-based composites prepared by dispersion strengthening of oxides, the Gr-modified Cu-Y2O3 achieves excellent comprehensive properties of high strength and high conductivity. The electrical conductivity of the Cu-Y2O3-Gr composite material is as high as 95.6%, and the Vickers hardness is as high as 120.8HV 0.1 .
Claims
1. A method for preparing a graphene-modified copper-based composite material, characterized in that: The specific steps include: Step 1: Molecular blending deposition (1) dissolving graphene powder in a graphene water dispersant containing sodium dodecylbenzene sulfonate and ultrasonically dispersing for 45-60 minutes; (2) adding copper nitrate solution to the above solution and continuing ultrasonic dispersion for 2 h to obtain a suspension; (3) drying the suspension obtained in step (2) to obtain a copper-loaded graphene composite powder; Step 2: Thermal Reduction The copper-graphene composite powder obtained in step 1 is placed in a high-temperature tube furnace and thermally reduced under a hydrogen atmosphere to obtain a Cu-Gr composite powder; Step 3: Solid phase reaction ball milling The Cu-Gr composite powder and Y2O3 powder prepared in step 2 are placed in a ball mill, and the ball mill is assembled in a vacuum glove box under an argon atmosphere. After the assembly is completed, the ball mill is placed in a planetary ball mill for ball milling at a ball milling speed of 300-350 r / min for 10-12 hours. After the ball milling is completed, the ball mill is taken out and ground to finally obtain a dispersed Cu-Y2O3-Gr composite powder; Step 4: Vacuum hot pressing sintering (1) The Cu-Y2O3-Gr composite powder obtained in step 3 is loaded into the assembled graphite mold, and then the mold is placed on a tray and placed in a vacuum hot pressing sintering furnace, a temperature measuring thermocouple is inserted, and the infrared thermometer is aligned, and the vacuuming procedure is started; (2) The sintering temperature and pressure process curve were set. The temperature was first raised to 600 °C and kept at this temperature for 5 min, then raised to 900 °C and kept at this temperature for 5 min, and then cooled to room temperature to obtain the Cu-Y2O3-Gr composite material.
2. A method for preparing a graphene-modified copper-based composite material according to claim 1, characterized in that: In the step 1, the graphene powder has a purity of 99%, a thickness of 3-10 nm, and a diameter of 7-12 μm, wherein the mass fraction of the added graphene powder is ≤1%.
3. A method for preparing a graphene-modified copper-based composite material as claimed in claim 1, characterized in that: The purity of sodium dodecylbenzene sulfonate in the step 1 is not less than 90%.
4. A method for preparing a graphene-modified copper-based composite material as claimed in claim 1, characterized in that: In the step 1, the purity of copper nitrate and graphene water dispersant is 100%, the concentration of copper nitrate solution is 3 mol / L, and the volume of graphene water dispersant added is equal to the volume of copper nitrate solution added.
5. A method for preparing a graphene-modified copper-based composite material as claimed in claim 1, characterized in that: The model of the high-temperature tube furnace for the thermal reduction treatment in step 2 is GSL-1200X. The specific process of thermal reduction is to raise the temperature to 550°C-600°C and keep it for 2 hours, then reduce it to 500°C and cool it with the furnace. The heating rate during the thermal reduction process is 10°C / min, and the cooling rate is 10°C / min.
6. A method for preparing a graphene-modified copper-based composite material according to claim 1, characterized in that: In the step three, the assembly of the ball milling jar is completed in a vacuum glove box to ensure a pure ball milling environment. The model of the vacuum glove box is ZKX, the planetary ball mill is a QM QX4 all-round planetary ball mill, and the ball milling process is carried out under the protection of an argon atmosphere. The ball milling jar and the ball milling medium are both made of cemented carbide, the ball milling speed is 300-350 r / min, the ball milling time is 10-12 hours, and the ball-to-material ratio is 5:
1.
7. A method for preparing a graphene-modified copper-based composite material according to claim 1, characterized in that: The purity of the Y2O3 powder in step 3 is 99.99% and the particle size is 0.5 μm.
8. A method for preparing a graphene-modified copper-based composite material according to claim 1, characterized in that: The sintering furnace model for vacuum hot pressing sintering in step 4 is FHP-828, the pre-pressing pressure is 10 MPa, the sintering temperature is 900° C., the sintering time is 5 min, and the final pressure is 50 MPa, wherein the heat preservation at 600° C. for 5 min is to remove the contained gas.
9. A method for preparing a graphene-modified copper-based composite material according to claim 1, characterized in that: The heating rate of vacuum hot pressing sintering in step 4 is 100° C. / min, and the cooling rate is 100° C. / min.
10. The method for preparing a graphene-modified copper-based composite material according to claim 1, characterized in that: The diameter of the graphite mold in step 4 is 30 mm.
Citation Information
Patent Citations
Graphene / silicon carbide reinforced copper-based composite material and preparation method thereof
CN111057899A
Preparation method of copper-based oxide dispersion strengthened Cu-Y2O3 composite material
CN114752838A