High thermal conductivity brake disc and preparation method thereof
By using specific chemical components and processes in the brake disc, a high-content graphite and pearlite structure is formed, which solves the problem of insufficient performance of existing brake discs under high temperature and wear, significantly improves thermal conductivity and wear resistance, and prolongs service life. longevity and enhanced braking safety.
Patent Information
- Application Number
- CN202211539718.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-02
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2042-12-02
AI Technical Summary
Existing automobile brake discs are prone to cracks, cracks and other defects under high temperature, thermal fatigue and wear conditions, and their thermal conductivity, heat resistance and anti-wear properties are insufficient, resulting in insufficient braking safety and service life.
High thermal conductivity brake discs using specific chemical composition ratios, including carbon, silicon, manganese, chromium, boron and other elements, are prepared through medium frequency induction furnace smelting and injection pouring processes to form a high-content graphite and pearlite structure to improve thermal conductivity. Thermal stability and wear resistance.
The thermal conductivity, thermal fatigue performance and wear resistance of the brake disc are significantly improved, the service life is extended, braking safety is enhanced, and normal production is achieved through reasonable processes.
Smart Images

Figure BDA0003976866350000051
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of brake disc preparation, and in particular relates to a high thermal conductivity brake disc and a preparation method thereof. Background Art
[0002] The principle of the brake system is to assemble the brake disc with the wheel hub, and generate huge friction through dry friction with the brake lining, converting the kinetic energy of the high-speed vehicle into heat energy. Sometimes it only takes a dozen seconds or even less for a car to brake from a speed of 100 km / h to a standstill. It can be seen that the brake system is under a huge load. The brake disc is an important component in the brake system. Its performance directly affects the braking effect. During the braking process, the brake disc is always under wear and friction. If the pressure is too high, it will deform or crack; secondly, braking is a continuous cycle, which makes the brake disc always in the process of alternating hot and cold, which is prone to fatigue cracks. Automobile brake discs are used under high temperature, thermal fatigue and wear conditions. The brake disc material should have good thermal conductivity, heat resistance, fatigue performance and wear resistance. At present, automobile brake discs are usually produced with high-strength gray cast iron, which has poor heat resistance and fatigue resistance. After wear during use, defects such as cracks and cracks are prone to occur. Summary of the invention
[0003] The technical problem to be solved by the present invention is to provide a high thermal conductivity brake disc with good thermal conductivity, high temperature strength, high temperature wear resistance and thermal fatigue resistance, which can significantly improve the safety reliability and service life of the brake disc; the present invention also provides a preparation method thereof with reasonable process.
[0004] The main chemical components and their weight percentages of the high thermal conductivity brake disc of the present invention are: 3.7-4.0% carbon, 0.6-1.2% silicon, 0.6-0.8% manganese, 0.1-0.3% chromium, 0.02-0.12% boron, and the rest are iron and inevitable impurities.
[0005] Carbon is a graphite-forming element, and a high carbon content is beneficial to improving thermal conductivity.
[0006] Silicon is a graphitization-promoting element, which is beneficial to the elimination of free cementite, but too high silicon content will reduce the pearlite content, strength and wear resistance.
[0007] Manganese promotes the formation of pearlite, but too high a content will cause segregation and reduce plasticity.
[0008] Chromium increases the pearlite content, making the cementite in the pearlite become chromium-containing cementite Fe(Cr)3C, which improves thermal stability, but too high manganese content will promote the formation of free cementite.
[0009] Both titanium and boron can promote the formation of carbides and borides, improving strength, tensile hardness, wear resistance and high temperature stability of the structure.
[0010] The method for preparing the high thermal conductivity brake disc of the present invention comprises the following steps:
[0011] (1) melting the main smelting materials of scrap steel and recycled materials and the smelting auxiliary material of carburizer in a medium frequency induction furnace;
[0012] (2) adding manganese alloy, chromium alloy and boron alloy into a medium frequency induction furnace for melting to obtain a molten liquid;
[0013] (3) Pour the molten metal into the casting ladle by flushing method to carry out in-stream inoculation and in-mold inoculation;
[0014] (4) After the incubation is completed, casting is performed to obtain a brake disc.
[0015] Preferably, the amount of scrap steel added to the main smelting material accounts for 40% of the total weight, the amount of recycled material added accounts for 60% of the total weight, and the amount of recarburizer added as a smelting auxiliary material is 2.3% of the weight of the main smelting material; the scrap steel is Q235 ordinary carbon structural steel, the recycled material is brake disc recycled material, and the recarburizer is a graphitized recarburizer with a carbon content of 98.5%.
[0016] Preferably, the manganese alloy is FeMn63, and its addition amount is 0.3% of the weight of the main smelting material; the chromium alloy is FeCr55C4-0, and its addition amount is 0.2% of the weight of the main smelting material; the boron alloy is FeB18C0.5A or FeB18C0.5B, and its addition amount is 0.5%-0.7% of the weight of the main smelting material.
[0017] Preferably, the inoculant is a silicon-barium-calcium-iron alloy, whose main chemical components and their weight percentages are: 60% silicon, 2% calcium, 1% aluminum, 3% barium, and the rest is iron and inevitable impurities. The amount of inoculant added is 0.3-0.4% of the weight of the smelting liquid.
[0018] Preferably, the inoculant is a silicon-zirconium alloy, the main chemical components and their weight percentages of which are: 65% silicon, 7% zirconium, and the rest iron and inevitable impurities. The amount of inoculant added is 0.05-0.1% of the weight of the smelting liquid.
[0019] Preferably, the melting temperature is 1480-1520°C and the pouring temperature is 1390-1410°C.
[0020] The prepared brake disc has a metallographic structure of: type A graphite>90%, and the rest is type C graphite; the matrix structure is: pearlite>95%, phosphorus eutectic<2%, and carbide<3%.
[0021] Compared with the prior art, the present invention has the following beneficial effects:
[0022] 1. The brake disc of the present invention has good mechanical properties, with a tensile strength of ≥170MPa and a hardness of ≥160HBW.
[0023] 2. The brake disc of the present invention has good thermal conductivity, high temperature strength, high temperature wear resistance and thermal fatigue resistance, which can significantly improve braking safety and service life.
[0024] 3. The method for preparing the brake disc of the present invention has reasonable process and can be realized by normal production equipment. DETAILED DESCRIPTION
[0025] The present invention will be further described below in conjunction with the embodiments.
[0026] It should be noted that all raw materials used in the examples are commercially available unless otherwise specified.
[0027] Example 1
[0028] The main chemical components and their weight percentages of the high thermal conductivity brake disc of the present invention are: 3.95% carbon, 0.98% silicon, 0.65% manganese, 0.25% chromium, 0.08% boron, and the rest are iron and inevitable impurities.
[0029] The preparation method is as follows:
[0030] (1) smelting the main materials of scrap steel and recycled materials and the auxiliary materials of recarburizer in a medium frequency induction furnace at a smelting temperature of 1480° C.
[0031] Among them, the amount of scrap steel added to the main smelting material accounts for 40% of the total weight, the amount of recycled materials added accounts for 60% of the total weight, and the amount of recarburizer added as a smelting auxiliary material is 2.3% of the weight of the main smelting material; the scrap steel is Q235 ordinary carbon structural steel, the recycled materials are brake disc recycled materials, and the recarburizer is a graphitized recarburizer with a carbon content of 98.5%;
[0032] (2) adding manganese alloy, chromium alloy and boron alloy into a medium frequency induction furnace for melting to obtain a molten liquid;
[0033] Among them, the manganese alloy is FeMn63, and its addition amount is 0.3% of the weight of the main smelting material; the chromium alloy is FeCr55C4-0, and its addition amount is 0.2% of the weight of the main smelting material; the boron alloy is FeB18C0.5A, and its addition amount is 0.5% of the weight of the main smelting material;
[0034] (3) The molten metal is poured into a casting ladle by the flushing method for in-stream inoculation and in-mold inoculation, and the composition of the molten metal is tested at the same time;
[0035] The inoculant is a silicon-barium-calcium-iron alloy, and its main chemical components and their weight percentages are: 60% silicon, 2% calcium, 1% aluminum, 3% barium, and the rest are iron and impurities. The amount of inoculant added is 0.3% of the weight of the smelting liquid;
[0036] The inoculant in the mold is a silicon-zirconium alloy, and its main chemical components and their weight percentages are: 65% silicon, 7% zirconium, and the rest are iron and impurities. The amount of inoculant added in the mold is 0.06% of the weight of the smelting liquid;
[0037] (4) After the molten liquid is tested to be qualified, pouring is carried out at a pouring temperature of 1390° C. to obtain a casting. The sand in the casting and the filling sand in the sand box are cleaned to obtain the brake disc of the present invention.
[0038] Example 2
[0039] The main chemical components and their weight percentages of the high thermal conductivity brake disc of the present invention are: 3.75% carbon, 1.15% silicon, 0.73% manganese, 0.28% chromium, 0.11% boron, and the rest are iron and inevitable impurities.
[0040] The preparation method is as follows:
[0041] (1) melting the main smelting materials of scrap steel and recycled materials and the smelting auxiliary material of carburizer in a medium frequency induction furnace at a melting temperature of 1520°C;
[0042] Among them, the amount of scrap steel added to the main smelting material accounts for 40% of the total weight, the amount of recycled materials added accounts for 60% of the total weight, and the amount of recarburizer added as a smelting auxiliary material is 2.3% of the weight of the main smelting material; the scrap steel is Q235 ordinary carbon structural steel, the recycled materials are brake disc recycled materials, and the recarburizer is a graphitized recarburizer with a carbon content of 98.5%;
[0043] (2) adding manganese alloy, chromium alloy and boron alloy into a medium frequency induction furnace for melting to obtain a molten liquid;
[0044] Among them, the manganese alloy is FeMn63, and its addition amount is 0.3% of the weight of the main smelting material; the chromium alloy is FeCr55C4-0, and its addition amount is 0.2% of the weight of the main smelting material; the boron alloy is FeB18C0.5B, and its addition amount is 0.7% of the weight of the main smelting material;
[0045] (3) The molten metal is poured into a casting ladle by the flushing method for in-stream inoculation and in-mold inoculation, and the composition of the molten metal is tested at the same time;
[0046] The inoculant is a silicon-barium-calcium-iron alloy, and its main chemical components and their weight percentages are: 60% silicon, 2% calcium, 1% aluminum, 3% barium, and the rest are iron and impurities. The amount of inoculant added is 0.4% of the weight of the smelting liquid;
[0047] The inoculant in the mold is a silicon-zirconium alloy, and its main chemical components and their weight percentages are: 65% silicon, 7% zirconium, and the rest are iron and impurities. The amount of inoculant added in the mold is 0.1% of the weight of the smelting liquid;
[0048] (4) After the molten liquid is tested to be qualified, pouring is carried out at a pouring temperature of 1410° C. to obtain a casting, and the sand in the casting and the filling sand in the sand box are cleaned to obtain the brake disc of the present invention.
[0049] Example 3
[0050] The main chemical components and their weight percentages of the high thermal conductivity brake disc of the present invention are: 3.80% carbon, 0.85% silicon, 0.78% manganese, 0.15% chromium, 0.05% boron, and the rest are iron and inevitable impurities.
[0051] The preparation method is as follows:
[0052] (1) melting the main materials of smelting scrap steel and recycled materials and the auxiliary materials of smelting carburizer in a medium frequency induction furnace at a melting temperature of 1500° C.
[0053] Among them, the amount of scrap steel added to the main smelting material accounts for 40% of the total weight, the amount of recycled materials added accounts for 60% of the total weight, and the amount of recarburizer added as a smelting auxiliary material is 2.3% of the weight of the main smelting material; the scrap steel is Q235 ordinary carbon structural steel, the recycled materials are brake disc recycled materials, and the recarburizer is a graphitized recarburizer with a carbon content of 98.5%;
[0054] (2) adding manganese alloy, chromium alloy and boron alloy into a medium frequency induction furnace for melting to obtain a molten liquid;
[0055] Among them, the manganese alloy is FeMn63, and its addition amount is 0.3% of the weight of the main smelting material; the chromium alloy is FeCr55C4-0, and its addition amount is 0.2% of the weight of the main smelting material; the boron alloy is FeB18C0.5A, and its addition amount is 0.6% of the weight of the main smelting material;
[0056] (3) The molten metal is poured into a casting ladle by the flushing method for in-stream inoculation and in-mold inoculation, and the composition of the molten metal is tested at the same time;
[0057] The inoculant is a silicon-barium-calcium-iron alloy, and its main chemical components and their weight percentages are: 60% silicon, 2% calcium, 1% aluminum, 3% barium, and the rest are iron and impurities. The amount of inoculant added is 0.35% of the weight of the smelting liquid;
[0058] The inoculant in the mold is a silicon-zirconium alloy, and its main chemical components and their weight percentages are: 65% silicon, 7% zirconium, and the rest are iron and impurities. The amount of inoculant added in the mold is 0.05% of the weight of the smelting liquid;
[0059] (4) After the molten liquid is tested to be qualified, pouring is carried out at a pouring temperature of 1400° C. to obtain a casting of a specified shape. The sand in the casting and the filling sand in the sand box are cleaned to obtain the brake disc of the present invention.
[0060] The brake discs prepared in Examples 1 to 3 were tested: metallographic structure: type A graphite>90%, the rest is type C graphite; matrix structure: pearlite>95%, phosphorus eutectic<2%, carbide<3%. At the same time, the performance of the brake disc was tested and compared with HT250, and the results are shown in Table 1.
[0061] From the comparison results, it can be seen that compared with ordinary HT250, the high thermal conductivity brake disc of the present invention has greatly improved thermal conductivity, increased crack cycle times, and greatly shortened crack length, thereby increasing the service life of the brake disc and reducing the probability of brake failure caused by brake overheating, which is beneficial to driving safety and meets the design requirements.
[0062] Table 1 Brake disc performance test data
[0063]
Claims
1. A method for preparing a high thermal conductivity brake disc, characterized in that: The main chemical components of the brake disc and their weight percentages are: carbon 3.7-4.0%, silicon 0.6-1.2%, manganese 0.6-0.8%, chromium 0.15-0.28%, boron 0.05-0.11%, and the rest are iron and unavoidable impurities; The method for preparing the high thermal conductivity brake disc comprises the following steps: (1) Melting the main smelting materials of scrap steel and recycled materials and the smelting auxiliary materials of carburizer in a medium frequency induction furnace; (2) adding manganese alloy, chromium alloy and boron alloy into a medium frequency induction furnace for smelting to obtain a molten liquid; (3) The molten metal is poured into the casting ladle by the flushing method for inoculation and in-mold inoculation; (4) After the incubation is completed, casting is performed to obtain the brake disc; The amount of scrap steel added as the main smelting material accounts for 40% of the total weight, and the amount of recycled materials added accounts for 60% of the total weight; The amount of carburizer added is 2.3% of the weight of the main smelting material; The amount of manganese alloy added is 0.3% of the weight of the main smelting material, the amount of chromium alloy added is 0.2% of the weight of the main smelting material; the amount of boron alloy added is 0.5%-0.7% of the weight of the main smelting material.
2. The method for preparing a high thermal conductivity brake disc according to claim 1, characterized in that: The amount of inoculant added is 0.3-0.4% of the weight of the smelting liquid.
3. The method for preparing a high thermal conductivity brake disc according to claim 2, characterized in that: The inoculant is a silicon-barium-calcium-iron alloy, and its main chemical components and their weight percentages are: 60% silicon, 2% calcium, 1% aluminum, 3% barium, and the rest are iron and inevitable impurities.
4. The method for preparing a high thermal conductivity brake disc according to claim 1, characterized in that: The amount of inoculant added to the mold is 0.05-0.1% of the weight of the smelting liquid.
5. The method for preparing a high thermal conductivity brake disc according to claim 4, characterized in that: The inoculant in the mold is a silicon-zirconium alloy, and its main chemical components and their weight percentages are: 65% silicon, 7% zirconium, and the rest are iron and inevitable impurities.
6. The method for preparing a high thermal conductivity brake disc according to claim 1, characterized in that: The melting temperature is 1480-1520℃ and the pouring temperature is 1390-1410℃.
Citation Information
Patent Citations
High-carbon low-silicon niobium-containing cast iron brake disc and preparation method thereof
CN104195423A
Production method of cylinder sleeve
CN106555104A
Brake disc for utility vehicles
EP1004789A2