Q690D hot-rolled steel strip with good bending performance and production method

By optimizing the chemical composition and process flow in the Q690D hot-rolled steel strip, ferrite + M/A island-like structure is formed, the deficiencies in bending performance of low alloy high-strength steel are solved, and high strength, toughness and easy welding are achieved It is suitable for lightweight automobiles and engineering machinery, reducing costs.

CN116288046BActive Publication Date: 2024-11-26TANGSHAN IRON & STEEL GROUP +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310122789.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-16
Publication Date
2024-11-26
Estimated Expiration
2043-02-16

AI Technical Summary

Technical Problem

Existing low alloy high strength steels lack good bending performance in applications, making it difficult to meet the needs of lightweight automotive structures and engineering machinery, especially to maintain high strength and toughness while saving costs.

Method used

The chemical composition is C: 0.06-0.10%, Mn: 1.60-1.85%, S≤0.006%, P≤0.020%, Si: 0.15-0.30%, Als: 0.030-0.040%, Ti: 0.080-0.150%, Cr: 0.15-0.30%, Nb: 0.04-0.08%, Mo: 0.15-0.25% of Q690D hot-rolled steel strip, and is subjected to converter smelting, LF furnace refining, slab continuous casting, heating, rough rolling, finishing rolling, cooling , winding and cooling processes to form a metallographic structure of ferrite + M/A island-shaped structure.

Benefits of technology

The high yield strength, tensile strength and impact toughness of the Q690D hot-rolled steel strip are achieved, ensuring its application in lightweight automotive structures and engineering machinery, with good welding performance and bending performance, and reducing construction costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116288046B_ABST
    Figure CN116288046B_ABST
Patent Text Reader

Abstract

The invention discloses a Q690D hot-rolled steel strip with good bending performance and a production method. The chemical composition and mass percentage of the hot-rolled steel strip are: C: 0.06-0.10%, Mn: 1.60-1.85%, S≤0.006%, P≤0.020%, Si: 0.15-0.30%, Als: 0.030-0.040%, Ti: 0.080-0.150%, Cr: 0.15-0.30%, Nb: 0.04-0.08%, Mo: 0.15-0.25%; the balance is Fe and unavoidable impurities. The production method includes converter smelting, LF furnace refining, slab continuous casting, heating, rough rolling, finish rolling, cooling, coiling and steel coil slow cooling processes. The hot-rolled steel strip obtained by the invention not only ensures strength, but also takes into account welding performance and bending performance, providing a good performance foundation for subsequent cold processing.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of metallurgy, and in particular relates to a Q690D hot-rolled steel strip with good bending performance and a production method thereof. Background Art

[0002] Due to its high strength, low-alloy high-strength steel can effectively save material consumption during application and reduce the pressure on resources, energy and the environment. Therefore, in recent years, the domestic demand for low-alloy high-strength steel has gradually increased, accounting for about 30% of steel production, and is widely used in many industries such as construction, engineering machinery, transportation, bridges and automobiles.

[0003] Low alloy steel and high strength steel have the characteristics of low alloy content and high product strength compared to ordinary carbon steel. Low alloy high strength steel often adopts micro-alloying composition design, and the total amount of alloy elements added generally does not exceed 5%. Controlled rolling and controlled cooling are used to exert the effects of alloy element solid solution strengthening and precipitation strengthening to obtain excellent strength and toughness.

[0004] With the continuous advancement of lightweight demand in the automotive, engineering machinery and transportation industries, the strength level of corresponding raw materials has been greatly improved, that is, the weight of steel is reduced as much as possible on the basis of achieving the same strength requirements. Steels with tensile strength above 700MPa are highly favored.

[0005] Low alloy high strength steel is usually divided into two types: non-quenched and tempered. The non-quenched and tempered state is mainly hot rolled. Since no heat treatment is performed, its tensile strength is generally less than 780MPa. Low alloy high strength steel after quenching and high temperature tempering is called quenched and tempered steel, and its yield strength can generally reach 780-1200MPa. Generally, due to the high cost and low utilization rate of heat treatment process, general steel enterprises do not use heat treatment process for hot rolled products used in general structures. Therefore, achieving higher yield strength of hot rolled products through composition and rolling process has broad market prospects. Summary of the invention

[0006] The technical problem to be solved by the present invention is to provide a Q690D hot-rolled steel strip with good bending performance and a production method thereof. The present invention is suitable for lightweight automobile structures and engineering machinery steels, and the obtained hot-rolled steel strip is suitable for automobile structures and engineering machinery steels, and has high strength and toughness, easy weldability and other characteristics while saving costs.

[0007] In order to solve the above technical problems, the technical solution adopted by the present invention is: a Q690D hot-rolled steel strip with good bending performance, the chemical composition of the hot-rolled steel strip and its mass percentage are: C: 0.06-0.10%, Mn: 1.60-1.85%, S≤0.006%, P≤0.020%, Si: 0.15-0.30%, Als: 0.030-0.040%, Ti: 0.080-0.150%, Cr: 0.15-0.30%, Nb: 0.04-0.08%, Mo: 0.15-0.25%; the balance is Fe and unavoidable impurities.

[0008] The hot-rolled steel strip of the present invention has a thickness of 6.0 to 15.0 mm and a width of 1200 to 1800 mm.

[0009] The metallographic structure of the hot-rolled steel strip of the present invention is ferrite+M / A island structure.

[0010] The hot-rolled steel strip of the present invention has a yield strength ReH of 740-840 MPa, a tensile strength Rm of 820-920 MPa, an elongation after fracture A≥20%, an impact toughness at -20°C≥90J, and no cracks when the bending center diameter is 2a.

[0011] Another object of the present invention is to provide a production method for the above-mentioned Q690D hot-rolled steel strip with good bending performance, the production method comprising converter smelting, LF furnace refining, slab continuous casting, heating, rough rolling, finishing rolling, cooling, coiling and slow cooling of steel coils; the rough rolling process is divided into two rolling mills for a total of 6 passes, adopting a 3+3 rough rolling mode, and the intermediate billet thickness is 45-55mm; the finishing rolling process is rolled into a steel strip with a thickness of 6.0-15.0mm through 7 passes of finishing rolling, the finishing rolling inlet temperature is 1020-1060°C, and the final rolling temperature is 840-910°C; the cooling process adopts laminar cooling and adopts ultra-fast cooling (closed) + intensive water cooling + air cooling mode, and the cooling rates of each section are 10-20°C / s, 50-60°C / s, and 10-20°C / s, respectively.

[0012] The converter smelting and LF furnace refining process of the present invention controls the chemical composition of the molten steel and its mass percentage content to be: C: 0.06-0.10%, Mn: 1.60-1.85%, S≤0.006%, P≤0.020%, Si: 0.15-0.30%, Als: 0.030-0.040%, Ti: 0.080-0.150%, Cr: 0.15-0.30%, Nb: 0.04-0.08%, Mo: 0.15-0.25%, and the balance is Fe and unavoidable impurities.

[0013] The heating process of the present invention is to heat the steel billet in a walking beam heating furnace, wherein the temperature of the steel billet heating soaking section is ≥1280°C, the soaking time is 40 to 45 minutes, and the total heating time is 180 to 230 minutes.

[0014] In the coiling process of the present invention, the coiling temperature is 590-650° C., and the hot-rolled steel strip is placed in a slow cooling pit for slow cooling for 24-36 hours after being coiled.

[0015] The Q690D hot-rolled steel strip product with good bending performance of the present invention refers to GB / T 1591-2018 for product standard; the product performance detection method standard refers to GB / T 228.1 (tensile test), GB / T232 (bending test), and GB / T 229 (impact test).

[0016] The beneficial effects of the above technical scheme are: 1. The chemical composition of the present invention is reasonably designed. By adding alloy elements such as Si, Nb, Ti, Mo, Cr, etc., the fine grain strengthening and precipitation strengthening of the alloy are fully utilized, and the grain structure is refined to improve the product strength. 2. The present invention reasonably designs the hot rolling heating system and cooling path, and the obtained hot-rolled steel strip is suitable for automobile structure and engineering machinery steel. While having high strength, it also ensures the welding performance and bending performance of the product, providing a good performance foundation for subsequent cold processing such as bending, punching, welding and other processes. 3. The metallographic structure of the ultra-high strength hot-rolled steel strip of the present invention is ferrite + M / A island structure, ReH: 740~840MPa, tensile strength Rm: 820~920MPa, elongation after fracture A≥20%, -20℃ impact toughness≥90J, no cracks when the bending core diameter is 2a; it is suitable for lightweight automobile structure and engineering machinery steel, and has high strength and toughness, easy weldability and other characteristics while saving construction costs. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 The metallographic structure diagram of the Q690D hot-rolled steel strip of Example 1;

[0018] Figure 2 This is the metallographic structure diagram of the Q690D hot-rolled steel strip of Example 2;

[0019] Figure 3 This is the metallographic structure diagram of the Q690D hot-rolled steel strip of Example 3;

[0020] Figure 4 This is the metallographic structure diagram of the Q690D hot-rolled steel strip of Example 4;

[0021] Figure 5 This is the metallographic structure diagram of the Q690D hot-rolled steel strip of Example 5;

[0022] Figure 6This is the metallographic structure diagram of the Q690D hot-rolled steel strip of Example 6;

[0023] Figure 7 The metallographic structure diagram of the Q690D rolled steel strip of Example 7;

[0024] Figure 8 This is the metallographic structure diagram of the Q690D hot-rolled steel strip of Example 8. Implementation

[0025] The present invention will be further described in detail below with reference to specific embodiments. Example 1

[0026] The non-quenched and tempered Q690D hot-rolled steel strip of this embodiment has a thickness of 6.0 mm and a width of 1200 mm. Its chemical composition and mass percentage are shown in Table 1.

[0027] The production method of Q690D hot-rolled steel strip in this embodiment includes the processes of converter smelting, LF furnace refining, slab continuous casting, heating, rough rolling, finish rolling, cooling, coiling and slow cooling of steel coils, and the specific process steps are as follows:

[0028] (1) Converter smelting, LF furnace refining and slab continuous casting process: control the chemical composition of molten steel to obtain qualified ingots;

[0029] (2) Heating process: Heating in a walking beam heating furnace, the temperature of the steel billet heating soaking section is 1320°C, the soaking time is 40 minutes, and the total heating time is 220 minutes;

[0030] (3) Rough rolling process: Two rough rolling mills are used for a total of 6 passes, using a 3+3 rough rolling mode, with an intermediate billet thickness of 45 mm;

[0031] (4) Finishing rolling process: After 7 passes of finishing rolling, the steel strip is rolled into a thickness of 6.0 mm, the finishing rolling inlet temperature is 1052°C, and the final rolling temperature is 880°C;

[0032] (5) Cooling process: ultra-fast cooling (off) + intensive water cooling + air cooling mode, the cooling rates of each section are 18℃ / s, 53℃ / s, and 12℃ / s respectively;

[0033] (6) Coiling process: the coiling temperature is 620℃, and the coiling is followed by slow cooling for 28h to obtain Q690D hot-rolled steel strip.

[0034] The mechanical properties of the Q690D hot-rolled steel strip in this embodiment are shown in Table 2; the metallographic structure of the hot-rolled steel strip is ferrite + M / A island structure, and the metallographic structure diagram is shown in Figure 1 . Example 2

[0035] The non-quenched and tempered Q690D hot-rolled steel strip in this embodiment has a thickness of 8.0 mm and a width of 1380 mm. Its chemical composition and mass percentage are shown in Table 1.

[0036] The production method of Q690D hot-rolled steel strip in this embodiment includes the processes of converter smelting, LF furnace refining, slab continuous casting, heating, rough rolling, finish rolling, cooling, coiling and slow cooling of steel coils, and the specific process steps are as follows:

[0037] (1) Converter smelting, LF furnace refining and slab continuous casting process: control the chemical composition of molten steel to obtain qualified ingots;

[0038] (2) Heating process: Heating in a walking beam heating furnace, the temperature of the steel billet heating soaking section is 1320°C, the soaking time is 42 minutes, and the total heating time is 190 minutes;

[0039] (3) Rough rolling process: Two rough rolling mills are used for a total of 6 passes, using a 3+3 rough rolling mode, with an intermediate billet thickness of 48 mm;

[0040] (4) Finishing rolling process: After 7 passes of finishing rolling, the steel strip is rolled into a thickness of 8.0 mm, the finishing rolling inlet temperature is 1037°C, and the final rolling temperature is 860°C;

[0041] (5) Cooling process: ultra-fast cooling (off) + intensive water cooling + air cooling mode, the cooling rates of each section are 16℃ / s, 50℃ / s, and 13℃ / s respectively;

[0042] (6) Coil-up process: the coil-up temperature is 620°C, and the steel is slowly cooled after coiling for 24 hours to obtain a Q690D hot-rolled steel strip.

[0043] The mechanical properties of the Q690D hot-rolled steel strip in this embodiment are shown in Table 2; the metallographic structure of the hot-rolled steel strip is ferrite + M / A island structure, and the metallographic structure diagram is shown in Figure 2 . Example 3

[0044] The non-quenched and tempered Q690D hot-rolled steel strip of this embodiment has a thickness of 10.0 mm and a width of 1250 mm. Its chemical composition and mass percentage are shown in Table 1.

[0045] The production method of Q690D hot-rolled steel strip in this embodiment includes the processes of converter smelting, LF furnace refining, slab continuous casting, heating, rough rolling, finish rolling, cooling, coiling and slow cooling of steel coils, and the specific process steps are as follows:

[0046] (1) Converter smelting, LF furnace refining and slab continuous casting process: control the chemical composition of molten steel to obtain qualified ingots;

[0047] (2) Heating process: Heating in a walking beam heating furnace, the temperature of the steel billet in the soaking zone is 1280°C, the soaking time is 45 minutes, and the total heating time is 180 minutes;

[0048] (3) Rough rolling process: Two rough rolling mills are used for a total of 6 passes, using a 3+3 rough rolling mode, with an intermediate billet thickness of 46 mm;

[0049] (4) Finishing rolling process: After 7 passes of finishing rolling, the steel strip is rolled into a thickness of 10.0 mm, the finishing rolling inlet temperature is 1020 °C, and the final rolling temperature is 840 °C;

[0050] (5) Cooling process: ultra-fast cooling (off) + intensive water cooling + air cooling mode, the cooling rates of each section are 20℃ / s, 57℃ / s, and 10℃ / s respectively;

[0051] (6) Coil-up process: the coil-up temperature is 650°C, and the steel is slowly cooled after coiling for 34 hours to obtain a Q690D hot-rolled steel strip.

[0052] The mechanical properties of the Q690D hot-rolled steel strip in this embodiment are shown in Table 2; the metallographic structure of the hot-rolled steel strip is ferrite + M / A island structure, and the metallographic structure diagram is shown in Figure 3 . Example 4

[0053] The non-quenched and tempered Q690D hot-rolled steel strip in this embodiment has a thickness of 12.0 mm and a width of 1440 mm. Its chemical composition and mass percentage are shown in Table 1.

[0054] The production method of Q690D hot-rolled steel strip in this embodiment includes the processes of converter smelting, LF furnace refining, slab continuous casting, heating, rough rolling, finish rolling, cooling, coiling and slow cooling of steel coils, and the specific process steps are as follows:

[0055] (1) Converter smelting, LF furnace refining and slab continuous casting process: control the chemical composition of molten steel to obtain qualified ingots;

[0056] (2) Heating process: Heating in a walking beam heating furnace, the temperature of the steel billet heating soaking section is 1310°C, the soaking time is 40 minutes, and the total heating time is 200 minutes;

[0057] (3) Rough rolling process: Two rough rolling mills are used for a total of 6 passes, using a 3+3 rough rolling mode, with an intermediate billet thickness of 50 mm;

[0058] (4) Finishing rolling process: After 7 passes of finishing rolling, the steel strip is rolled into a thickness of 12.0 mm, the finishing rolling inlet temperature is 1035°C, and the final rolling temperature is 860°C;

[0059] (5) Cooling process: ultra-fast cooling (off) + intensive water cooling + air cooling mode, the cooling rates of each section are 17℃ / s, 60℃ / s, and 15℃ / s respectively;

[0060] (6) Coil-up process: the coil-up temperature is 590°C, and the steel is slowly cooled after coiling for 26 hours to obtain a Q690D hot-rolled steel strip.

[0061] The mechanical properties of the Q690D hot-rolled steel strip in this embodiment are shown in Table 2; the metallographic structure of the hot-rolled steel strip is ferrite + M / A island structure, and the metallographic structure diagram is shown in Figure 4 . Example 5

[0062] The non-quenched and tempered Q690D hot-rolled steel strip of this embodiment has a thickness of 14.0 mm and a width of 1560 mm. Its chemical composition and mass percentage are shown in Table 1.

[0063] The production method of Q690D hot-rolled steel strip in this embodiment includes the processes of converter smelting, LF furnace refining, slab continuous casting, heating, rough rolling, finish rolling, cooling, coiling and slow cooling of steel coils, and the specific process steps are as follows:

[0064] (1) Converter smelting, LF furnace refining and slab continuous casting process: control the chemical composition of molten steel to obtain qualified ingots;

[0065] (2) Heating process: Heating in a walking beam heating furnace, the temperature of the steel billet in the soaking section is 1280°C, the soaking time is 42 minutes, and the total heating time is 230 minutes;

[0066] (3) Rough rolling process: Two rough rolling mills are used for a total of 6 passes, using a 3+3 rough rolling mode, with an intermediate billet thickness of 50 mm;

[0067] (4) Finishing rolling process: After 7 passes of finishing rolling, the steel strip is rolled into a thickness of 14.0 mm, the finishing rolling inlet temperature is 1060°C, and the final rolling temperature is 890°C;

[0068] (5) Cooling process: ultra-fast cooling (off) + intensive water cooling + air cooling mode, the cooling rates of each section are 18℃ / s, 55℃ / s, and 20℃ / s respectively;

[0069] (6) Coil-up process: the coil-up temperature is 600°C, and the steel is slowly cooled after coiling for 32 hours to obtain Q690D hot-rolled steel strip.

[0070] The mechanical properties of the Q690D hot-rolled steel strip in this embodiment are shown in Table 2; the metallographic structure of the hot-rolled steel strip is ferrite + M / A island structure, and the metallographic structure diagram is shown in Figure 5 . Example 6

[0071] The non-quenched and tempered Q690D hot-rolled steel strip of this embodiment has a thickness of 10.0 mm and a width of 1800 mm. Its chemical composition and mass percentage are shown in Table 1.

[0072] The production method of Q690D hot-rolled steel strip in this embodiment includes the processes of converter smelting, LF furnace refining, slab continuous casting, heating, rough rolling, finish rolling, cooling, coiling and slow cooling of steel coils, and the specific process steps are as follows:

[0073] (1) Converter smelting, LF furnace refining and slab continuous casting process: control the chemical composition of molten steel to obtain qualified ingots;

[0074] (2) Heating process: Heating in a walking beam heating furnace, the temperature of the steel billet heating soaking section is 1300°C, the soaking time is 43 minutes, and the total heating time is 220 minutes;

[0075] (3) Rough rolling process: Two rough rolling mills are used for a total of 6 passes, using a 3+3 rough rolling mode, with an intermediate billet thickness of 47 mm;

[0076] (4) Finishing rolling process: After 7 passes of finishing rolling, the steel strip is rolled into a thickness of 10.0 mm, the finishing rolling inlet temperature is 1055°C, and the final rolling temperature is 910°C;

[0077] (5) Cooling process: ultra-fast cooling (off) + intensive water cooling + air cooling mode, the cooling rates of each section are 12℃ / s, 54℃ / s, and 17℃ / s respectively;

[0078] (6) Coil-up process: the coil-up temperature is 610°C, and the steel is slowly cooled after coiling for 35 hours to obtain a Q690D hot-rolled steel strip.

[0079] The mechanical properties of the Q690D hot-rolled steel strip in this embodiment are shown in Table 2; the metallographic structure of the hot-rolled steel strip is ferrite + M / A island structure, and the metallographic structure diagram is shown in Figure 6 . Example 7

[0080] The non-quenched and tempered Q690D hot-rolled steel strip of this embodiment has a thickness of 15.0 mm and a width of 1660 mm. Its chemical composition and mass percentage are shown in Table 1.

[0081] The production method of Q690D hot-rolled steel strip in this embodiment includes the processes of converter smelting, LF furnace refining, slab continuous casting, heating, rough rolling, finish rolling, cooling, coiling and slow cooling of steel coils, and the specific process steps are as follows:

[0082] (1) Converter smelting, LF furnace refining and slab continuous casting process: control the chemical composition of molten steel to obtain qualified ingots;

[0083] (2) Heating process: Heating in a walking beam heating furnace, the temperature of the steel billet heating soaking section is 1290°C, the soaking time is 45 minutes, and the total heating time is 200 minutes;

[0084] (3) Rough rolling process: Two rough rolling mills are used for a total of 6 passes, using a 3+3 rough rolling mode, with an intermediate billet thickness of 55 mm;

[0085] (4) Finishing rolling process: After 7 passes of finishing rolling, the steel strip is rolled into a thickness of 15.0 mm, the finishing rolling inlet temperature is 1046°C, and the final rolling temperature is 850°C;

[0086] (5) Cooling process: ultra-fast cooling (off) + intensive water cooling + air cooling mode, the cooling rates of each section are 10℃ / s, 52℃ / s, and 18℃ / s respectively;

[0087] (6) Coiling process: the coiling temperature is 600°C, and the steel is slowly cooled after coiling for 36 hours to obtain Q690D hot-rolled steel strip.

[0088] The mechanical properties of the Q690D hot-rolled steel strip in this embodiment are shown in Table 2; the metallographic structure of the hot-rolled steel strip is ferrite + M / A island structure, and the metallographic structure diagram is shown in Figure 7 . Example 8

[0089] The non-quenched and tempered Q690D hot-rolled steel strip in this embodiment has a thickness of 8.0 mm and a width of 1720 mm. Its chemical composition and mass percentage are shown in Table 1.

[0090] The production method of Q690D hot-rolled steel strip in this embodiment includes the processes of converter smelting, LF furnace refining, slab continuous casting, heating, rough rolling, finish rolling, cooling, coiling and slow cooling of steel coils, and the specific process steps are as follows:

[0091] (1) Converter smelting, LF furnace refining and slab continuous casting process: control the chemical composition of molten steel to obtain qualified ingots;

[0092] (2) Heating process: Heating in a walking beam heating furnace, the temperature of the steel billet in the soaking zone is 1310°C, the soaking time is 43 minutes, and the total heating time is 180 minutes;

[0093] (3) Rough rolling process: Two rough rolling mills are used for a total of 6 passes, using a 3+3 rough rolling mode, with an intermediate billet thickness of 52 mm;

[0094] (4) Finishing rolling process: After 7 passes of finishing rolling, the steel strip is rolled into a thickness of 6.0 mm. The finishing rolling inlet temperature is 1028°C and the final rolling temperature is 870°C.

[0095] (5) Cooling process: ultra-fast cooling (off) + intensive water cooling + air cooling mode, the cooling rates of each section are 13℃ / s, 58℃ / s, and 16℃ / s respectively;

[0096] (6) Coiling process: the coiling temperature is 640°C, and after coiling, slow cooling is performed for 30 hours to obtain Q690D hot-rolled steel strip.

[0097] The mechanical properties of the Q690D hot-rolled steel strip in this embodiment are shown in Table 2; the metallographic structure of the hot-rolled steel strip is ferrite + M / A island structure, and the metallographic structure diagram is shown in Figure 8 .

[0098] Table 1 Chemical composition and mass percentage of hot-rolled steel strips of Examples 1-8 (%)

[0099]

[0100] Table 2 Mechanical properties of Q690D hot-rolled steel strips of Examples 1-8

[0101]

[0102] The above embodiments are only used to illustrate rather than limit the technical solutions of the present invention. Although the present invention is described in detail with reference to the above embodiments, those skilled in the art should understand that the present invention can still be modified or replaced by equivalents. Any modification or partial replacement that does not depart from the spirit and scope of the present invention should be included in the scope of the claims of the present invention.

Claims

1. A Q690D hot-rolled steel strip with good bending performance, characterized in that: The chemical composition and mass percentage of the hot-rolled steel strip are: C: 0.06-0.10%, Mn: 1.60-1.85%, S≤0.006%, P≤0.020%, Si: 0.15-0.30%, Als: 0.030-0.040%, Ti: 0.080-0.150%, Cr: 0.15-0.30%, Nb: 0.04-0.08%, Mo: 0.15-0.25%; the balance is Fe and unavoidable impurities; The hot-rolled steel strip has a yield strength ReH of 740-840 MPa, a tensile strength Rm of 820-920 MPa, and no cracks when the bending center diameter is 2a; The metallographic structure of the hot-rolled steel strip is ferrite + M / A island structure; A production method of a Q690D hot-rolled steel strip with good bending performance comprises converter smelting, LF furnace refining, slab continuous casting, heating, rough rolling, finish rolling, cooling, coiling and slow cooling of steel coils; the rough rolling process is divided into two rolling mills for a total of 6 rolling passes, adopts a 3+3 rough rolling mode, and the thickness of the intermediate billet is 45-55 mm; the finish rolling process is rolled into a steel strip with a thickness of 6.0-15.0 mm through 7 finish rolling passes, the finish rolling inlet temperature is 1020-1060°C, and the final rolling temperature is 840-910°C; the cooling process adopts laminar cooling and adopts an ultra-fast cooling + intensive water cooling + air cooling mode, and the cooling rates of each section are 10-20°C / s, 50-60°C / s, and 10-20°C / s respectively; the coiling process has a coiling temperature of 590-650°C.

2. The Q690D hot-rolled steel strip with good bending performance according to claim 1, characterized in that: The hot-rolled steel strip has a thickness of 6.0 to 15.0 mm and a width of 1200 to 1800 mm.

3. The Q690D hot-rolled steel strip with good bending performance according to claim 1 or 2, characterized in that: The hot-rolled steel strip has a yield strength ReH of 740-840 MPa, a tensile strength Rm of 820-920 MPa, an elongation after fracture A≥20%, an impact toughness at -20°C≥90J, and no cracks when the bending center diameter is 2a.

4. A method for producing a Q690D hot-rolled steel strip with good bending performance according to any one of claims 1 to 3, characterized in that: The production method comprises converter smelting, LF furnace refining, slab continuous casting, heating, rough rolling, finish rolling, cooling, coiling and slow cooling of steel coils; the rough rolling process is divided into two rolling mills for a total of 6 rolling passes, adopts a 3+3 rough rolling mode, and the thickness of the intermediate billet is 45-55 mm; the finish rolling process is rolled into a steel strip with a thickness of 6.0-15.0 mm through 7 finish rolling passes, the finish rolling inlet temperature is 1020-1060°C, and the final rolling temperature is 840-910°C; the cooling process adopts laminar cooling and adopts an ultra-fast cooling + intensive water cooling + air cooling mode, and the cooling rates of each section are 10-20°C / s, 50-60°C / s, and 10-20°C / s respectively; the coiling process has a coiling temperature of 590-650°C.

5. The method for producing a Q690D hot-rolled steel strip with good bending performance according to claim 4, characterized in that: The heating process is carried out by heating in a walking beam heating furnace, the temperature of the steel billet heating soaking section is ≥1280°C, the soaking time is 40 to 45 minutes, and the total heating time is 180 to 230 minutes.

6. The method for producing a Q690D hot-rolled steel strip with good bending performance according to claim 4, characterized in that: In the coiling process, the hot rolled steel strip is placed in a slow cooling pit for slow cooling for 24 to 36 hours after being coiled.