A method for preparing ultra-thin strippable copper
By plasma cleaning and high-energy ion implantation of the carrier polymer, combined with the preparation of strength metal and carrier polymer, the porosity and uniformity problems of ultra-thin copper foil were solved, and high density and high peel strength were achieved. Preparation of extremely thin copper foil.
Patent Information
- Application Number
- CN202310221554.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-09
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2043-03-09
AI Technical Summary
It is difficult to effectively prepare ultra-thin copper foil with a thickness less than 3 μm using existing technology. There are many pores, poor uniformity of the film layer, and difficulty in controlling the bonding strength between the polymer carrier and ultra-thin copper, which affects product quality.
By performing roll-to-roll plasma cleaning and high-energy ion implantation on the carrier polymer, a hybrid structure of unidirectional bonding strength metal and carrier polymer is formed, and extremely thin copper is deposited on the surface to ensure that the bonding strength is between 0.1 and 0.2N/ cm range to improve peel strength and density.
It achieves high density and uniformity of extremely thin copper foil, with surface roughness less than 0.2μm, high folding resistance, low porosity, small consumption factor and low water absorption, breaking through the bottleneck of traditional preparation methods and suitable for large-scale applications Production.
Smart Images

Figure CN116288161B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of copper foil preparation, and in particular to a method for preparing extremely thin strippable copper. Background Art
[0002] Copper foil can be divided into several categories according to its thickness: thick copper foil, conventional copper foil, thin copper foil, ultra-thin copper foil, and ultra-thin copper foil. Among them, ultra-thin copper foil refers to copper foil with a thickness of less than 4μm. Ultra-thin copper foil is mainly used in the field of lithium-ion batteries for new energy vehicles. At present, the application ratio of 8μm copper foil in lithium-ion batteries is high. The use of ultra-thin copper foil can increase the battery energy density by at least 8%. However, it is difficult to prepare ultra-thin copper foil using the traditional method of calendering. The ultra-thin copper foil prepared by electrolysis has key technical problems such as many pores and poor film uniformity.
[0003] The preparation of ultra-thin strippable copper has always been a technical bottleneck in the industry; 1) Due to its thickness, ultra-thin copper is very prone to scratches, breakages, and tears on the surface, so it requires a polymer carrier, and the bonding strength between the polymer carrier and the ultra-thin copper cannot be too high or too low. The bonding strength needs to be between 0.1 and 0.2N. If it is too high, it will make the ultra-thin copper difficult to separate, and if it is too low, the ultra-thin copper will fall off and cause wrinkling and other problems, which greatly affects the quality of the ultra-thin copper; 2) Because it is extremely thin, holes are very easy to form during the copper growth process, resulting in a decrease in density and low product quality.
[0004] Therefore, obtaining an ultra-thin copper with few pores, good film uniformity and a thickness of less than 3 μm is a technical problem that urgently needs to be solved. Summary of the invention
[0005] The object of the present invention is to provide a method for preparing ultra-thin strippable copper. The present invention cleans the carrier polymer and then performs high-energy ion implantation treatment, thereby improving the peel strength between the unidirectional bonding strength metal and the carrier polymer while ensuring that the bonding strength between the unidirectional bonding strength metal and the copper foil is 0.1 to 0.2 N / cm.
[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0007] The present invention provides a method for preparing ultra-thin strippable copper, comprising the following steps:
[0008] 1) performing roll-to-roll plasma cleaning on the carrier polymer to obtain a cleaned carrier polymer;
[0009] 2) performing high-energy ion implantation treatment on the cleaned carrier polymer to obtain an ion-implanted carrier polymer;
[0010] The high energy ion implantation process is to implant elements using a high energy ion beam with an energy of 10 to 50 keV, with an implantation depth of 10 to 50 nm and an implantation dose of 1×10 15 ~1×10 16 / cm 2 , the surface roughness of the carrier polymer after injection is 0.01-0.1 μm;
[0011] 3) depositing a one-way bonding strength metal on the ion-implanted carrier polymer to obtain a carrier polymer with one-way bonding strength metal deposited thereon;
[0012] 4) Deposit extremely thin copper on the surface of the carrier polymer with unidirectional bonding strength metal deposition to obtain extremely thin and strippable copper.
[0013] Furthermore, the plasma cleaning in step 1) includes sequentially performing Penning ion source cleaning, Kaufman ion source cleaning, and cold cathode Hall source cleaning.
[0014] Furthermore, the voltage of the Penning ion source cleaning is 20-40 kV, the time is 1-5 min, and the oxygen flow rate is 10-50 sccm.
[0015] Furthermore, the voltage of the Kaufman ion source cleaning is 10-20 kV, the time is 1-5 min, and the oxygen flow rate is 10-50 sccm.
[0016] Furthermore, the voltage of the cold cathode Hall source cleaning is 0.5-1 kV, the time is 1-5 min, the argon gas flow rate is 10-50 sccm, and the roughness of the carrier polymer after cleaning is 0.1-0.4 μm.
[0017] Furthermore, the elements in step 2) include one or more of Fe, Ni, Co, N and O.
[0018] Furthermore, in the step 3), a low-energy ion beam is used to deposit a unidirectional bonding strength metal, the deposition thickness is 10-100 nm, the porosity of the metal film layer is ≤5%, and the roughness of the metal film layer is 0.01-0.1 μm.
[0019] Furthermore, the unidirectional bonding strength metal in step 3) includes one or more of Ti, Zr and Mo.
[0020] Furthermore, in the step 4), low-energy ion beam and electron beam evaporation are used to deposit active thin copper. During the low-energy ion beam deposition process, the current is 90-200A, the beam current is >600mA, and the deposition rate is ≥10nm / min; during the electron beam evaporation process, the power is ≥30kW, the deposition rate is ≤5μm / min, and the roll-to-roll speed is ≥3m / min.
[0021] Beneficial effects of the present invention:
[0022] 1. The present invention provides a method for preparing ultra-thin strippable copper, which forms a mixed structure with the carrier polymer matrix and the injected ions by injecting high-energy ions into the carrier polymer, and the bonding strength between the mixed structure and the base layer and between the mixed structure and the subsequently formed copper film layer is very good, thereby enhancing the anti-peeling strength.
[0023] 2. The present invention adopts a gas ion source to clean the carrier polymer. The treated carrier polymer has good physical and chemical stability and can be directly wiped with a wet towel and some neutral detergent or washed with water. The physical and chemical properties of the carrier polymer itself are not affected after washing. The Hall ion source is used to clean the carrier polymer to form a micro-etched nanostructure on the surface of the carrier polymer, so that the treated carrier polymer has a hydrophilic structure, the specific surface area is increased, and the surface energy can be greatly improved.
[0024] 3. The ultra-thin peelable copper prepared by the preparation method provided by the present invention has a unidirectional bonding strength between the metal and the carrier polymer of ≥0.7N / cm, and a bonding strength between the metal and the copper foil of 0.1-0.2N / cm.
[0025] 4. The ultra-thin peelable copper prepared by the present invention has good density, the thickness of the copper foil is 1-3 μm, the surface roughness is 0.05-0.2 μm, the thickness uniformity difference is less than 8% within a width of 500 mm, the folding times of the copper foil is ≥1500 times, the consumption factor is <0.04, the water absorption rate is <4%, and the extended tear strength is >4N / mm, breaking through the bottleneck of the prior art.
[0026] 5. The preparation method provided by the present invention can be promoted in polymer surface treatment. The equipment has a long service life and low cost, can realize large-scale roll-to-roll production, and can simultaneously take into account the surface resistivity, surface roughness, water absorption and tensile strength of the polymer. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 It is a line graph of the one-way bonding strength of the ultra-thin strippable copper obtained in Examples 1 to 4 of the present invention, the bonding strength between the metal and the carrier polymer, and the one-way bonding strength between the metal and the copper foil, wherein the abscissa represents Examples 1 to 4;
[0028] Figure 2 This is a graph of the porosity of copper foil after depositing copper foil in Examples 1 to 4 of the present invention, wherein the abscissa represents Examples 1 to 4. DETAILED DESCRIPTION
[0029] The present invention provides a method for preparing ultra-thin strippable copper, comprising the following steps:
[0030] 1) performing roll-to-roll plasma cleaning on the carrier polymer to obtain a cleaned carrier polymer;
[0031] 2) performing high-energy ion implantation treatment on the cleaned carrier polymer to obtain an ion-implanted carrier polymer;
[0032] The high energy ion implantation process is to implant elements using a high energy ion beam with an energy of 10 to 50 keV, with an implantation depth of 10 to 50 nm and an implantation dose of 1×10 15 ~1×10 16 / cm 2 , the surface roughness of the carrier polymer after injection is 0.01-0.1 μm;
[0033] 3) depositing a one-way bonding strength metal on the ion-implanted carrier polymer to obtain a carrier polymer with one-way bonding strength metal deposited thereon;
[0034] 4) Deposit extremely thin copper on the surface of the carrier polymer with unidirectional bonding strength metal deposition to obtain extremely thin and strippable copper.
[0035] In the present invention, the plasma cleaning in step 1) includes sequentially performing Penning ion source cleaning, Kaufman ion source cleaning, and cold cathode Hall source cleaning.
[0036] In the present invention, the voltage of the Penning ion source cleaning is 20 to 40 kV, preferably 22 to 38 kV, and more preferably 24 to 36 kV; the time of the Penning ion source cleaning is 1 to 5 min, preferably 2 to 4 min, and more preferably 3 min; the oxygen flow rate of the Penning ion source cleaning is 10 to 50 sccm, preferably 15 to 45 sccm, and more preferably 20 to 40 sccm.
[0037] In the present invention, the oxygen ion energy generated by the Penning ion source is relatively high, which facilitates the combination of O and H to form hydroxyl radicals and realize the embedding of oxygen. The proportion of hydroxyl radicals on the surface of the carrier polymer cleaned by the Penning ion source is ≥10%.
[0038] In the present invention, the voltage of the Kaufman ion source cleaning is 10-20 kV, preferably 12-18 kV, and more preferably 14-16 kV; the time of the Kaufman ion source cleaning is 1-5 min, preferably 2-4 min, and more preferably 3 min; the oxygen flow rate of the Kaufman ion source cleaning is 10-50 sccm, preferably 15-45 sccm, and more preferably 20-40 sccm.
[0039] In the present invention, the carrier polymer is cleaned by Kaufman ion source, and the surface resistance is less than 10 16Ω, O and C form a bond, which is conducive to the increase of surface energy and realizes the addition of oxygen. 16 Ω, the Penning ion source should be cleaned again, because the higher the resistance, the less CO bonds, OH groups and C formed on the surface, which is directly related to the surface hydrophilicity of the polymer.
[0040] In the present invention, the voltage for cleaning the cold cathode Hall source is 0.5-1 kV, preferably 0.6-0.9 kV, and more preferably 0.7-0.8 kV; the time for cleaning the cold cathode Hall source is 1-5 min, preferably 2-4 min, and more preferably 3 min; the argon gas flow rate for cleaning the cold cathode Hall source is 10-50 sccm, preferably 15-45 sccm, and more preferably 20-40 sccm; the roughness of the carrier polymer after cleaning the cold cathode Hall source is 0.1-0.4 μm, preferably 0.2-0.3 μm, and more preferably 0.25 μm.
[0041] In the present invention, the carrier polymer is cleaned by cold cathode Hall source, Ar ions are beneficial to the extraction of hydrogen, and can also micro-etch the surface of the carrier polymer. The carrier polymer cleaned by cold cathode Hall source realizes the extraction of hydrogen, and the surface roughness is 0.1-0.4μm. If the roughness is too small, the surface energy is low, the hydrophilicity is poor, and the bonding strength is not high; if the roughness is too large, the high-frequency loss is too large during high-frequency transmission. Therefore, when the roughness is greater than 0.4μm or less than 0.1μm, the cold cathode Hall source needs to be cleaned again. The control of roughness is achieved by adjusting the air intake, energy, etc. Any mismatch of parameters may result in substandard resistance, roughness, water absorption, hydrophilicity and surface energy.
[0042] After surface cleaning, the dielectric constant of the carrier polymer is greater than 3.0, the surface moisture absorption rate is greater than 10%, the surface resistance is greater than 1015Ω, the surface roughness is 0.1-0.4μm, the hydrophilic angle is 40-800, and the high-frequency dielectric loss (5GHz) is ≤0.004.
[0043] The steps of Penning ion source cleaning (1), Kaufman ion source cleaning (2), and cold cathode Hall source cleaning (3) in the present invention can be repeated. If the requirements cannot be met, the process can return to (1) and repeat (1) to (3) for plasma cleaning until the requirements are met.
[0044] In the present invention, the elements in step 2) include one or more of Fe, Ni, Co, N and O, preferably include one or more of Fe, Ni, Co and N, and more preferably include one or more of Fe, Co and N.
[0045] In the present invention, in the step 3), a low-energy ion beam is used to deposit a unidirectional bonding strength metal, and the deposition thickness is 10 to 100 nm, preferably 20 to 90 nm, and more preferably 30 to 80 nm; the porosity of the metal film layer is ≤5%, preferably the porosity of the metal film layer is ≤4.5%, and more preferably the porosity of the metal film layer is ≤4%; the roughness of the metal film layer is 0.01 to 0.1 μm, preferably 0.03 to 0.08 μm, and more preferably 0.05 to 0.06 μm.
[0046] In the present invention, after the one-way bonding strength metal is deposited on the carrier polymer, the bonding strength of the one-way bonding strength metal with the carrier polymer is ≥0.7 N / cm, and the bonding strength with the copper foil is 0.1-0.2 N / cm.
[0047] In the present invention, the one-way bonding strength metal in step 3) includes one or more of Ti, Zr and Mo, preferably the one-way bonding strength metal includes Ti and / or Zr, and more preferably the one-way bonding strength metal includes Ti.
[0048] In the present invention, in the step 4), low-energy ion beam and electron beam evaporation are used to deposit active thin copper. During the low-energy ion beam deposition process, the current is 90-200A, preferably 100-190A, and more preferably 110-180A; the beam current is >600mA, preferably the beam current is >650mA, and more preferably the beam current is >700mA; the deposition rate is ≥10nm / min, preferably ≥12nm / min, and more preferably ≥13nm / min; during the electron beam evaporation process, the power is ≥30kW, preferably the power is ≥32kW, and more preferably the power is ≥34kW; the deposition rate is ≤5μm / min, preferably ≤4.5μm / min, and more preferably ≤4μm / min; the roll-to-roll speed is ≥3m / min, preferably the roll-to-roll speed is ≥4m / min, and more preferably the roll-to-roll speed is ≥5m / min.
[0049] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.
[0050] Example 1
[0051] 1) The carrier polymer is not subjected to roll-to-roll plasma cleaning;
[0052] 2) Use a 50 keV high energy ion beam to implant Fe, Ni, and Co elements into the carrier polymer (where the molar ratio of Fe, Ni, and Co is 3:5:2). The implantation depth is 50 nm and the implantation dose is 1×10 15 / cm 2, an ion implantation carrier polymer is obtained, and the surface roughness of the ion implantation carrier polymer is 0.05 μm;
[0053] 3) using a low-energy ion beam to deposit unidirectional bonding strength metal Ti on the surface of the ion-implanted carrier polymer to obtain a carrier polymer with unidirectional bonding strength Ti, the deposition thickness of Ti is 10 nm, the porosity of the Ti film layer is 5%, and the roughness of the Ti film layer is 0.06 μm;
[0054] 4) Low-energy ion beam and electron beam evaporation were used to deposit extremely thin copper on the surface of a carrier polymer with single-unit bonding strength Ti. During the low-energy ion beam deposition process, the current was 90A, the beam current was 600mA, and the deposition rate was 10nm / min. During the electron beam evaporation process, the power was 30kW, the deposition rate was 5μm / min, the roll-to-roll speed was 3m / min, the thickness of the copper foil was 3μm, and the surface roughness was 0.1μm, obtaining extremely thin and strippable copper.
[0055] Example 2
[0056] 1) The carrier polymer was sequentially cleaned by Penning ion source, Kaufman ion source and cold cathode Hall source roll-to-roll cleaning, wherein the voltage of Penning ion source cleaning was 50 kV, the time was 5 min, and the oxygen flow rate was 10 sccm, the voltage of Kaufman ion source cleaning was 10 kV, the time was 1 min, the oxygen flow rate was 50 sccm, and the voltage of cold cathode Hall source cleaning was 0.5 kV, the time was 3 min, and the argon flow rate was 35 sccm. After cleaning, the roughness of the carrier polymer was 0.4 μm;
[0057] 2) The cleaned carrier polymer is not subjected to high energy ion implantation treatment;
[0058] 3) using a low-energy ion beam to deposit unidirectional bonding strength metal Ti on the surface of the cleaned carrier polymer to obtain a carrier polymer with unidirectional bonding strength Ti, the deposition thickness of Ti is 30 nm, the porosity of the Ti film layer is 3%, and the roughness of the Ti film layer is 0.3 μm;
[0059] 4) Low-energy ion beam and electron beam evaporation were used to deposit extremely thin copper on the surface of a carrier polymer with single-unit bonding strength Ti. During the low-energy ion beam deposition process, the current was 150A, the beam current was 800mA, and the deposition rate was 12nm / min; during the electron beam evaporation process, the power was 40kW, the deposition rate was 3μm / min, the roll-to-roll speed was 5m / min, the thickness of the copper foil was 2μm, and the surface roughness was 0.15μm, obtaining extremely thin and strippable copper.
[0060] Example 3
[0061] 1) The carrier polymer was sequentially cleaned by Penning ion source, Kaufman ion source and cold cathode Hall source roll-to-roll cleaning, wherein the voltage of Penning ion source cleaning was 35 kV, the time was 3 min, the oxygen flow rate was 50 sccm, the voltage of Kaufman ion source cleaning was 20 kV, the time was 5 min, the oxygen flow rate was 10 sccm, the voltage of cold cathode Hall source cleaning was 1 kV, the time was 1 min, the argon flow rate was 10 sccm, and the roughness of the carrier polymer after cleaning was 0.25 μm;
[0062] 2) The Fe element was implanted into the carrier polymer using a high-energy ion beam with an energy of 10 keV. The implantation depth was 40 nm and the implantation dose was 1×10 16 / cm 2 , an ion implantation carrier polymer is obtained, and the surface roughness of the ion implantation carrier polymer is 0.08 μm;
[0063] 3) using a low-energy ion beam to deposit unidirectional bonding strength metal Ti on the surface of the ion-implanted carrier polymer to obtain a carrier polymer with unidirectional bonding strength Ti, the deposition thickness of Ti is 50 nm, the porosity of the Ti film layer is 5%, and the roughness of the Ti film layer is 0.1 μm;
[0064] 4) Low-energy ion beam and electron beam evaporation were used to deposit extremely thin copper on the surface of a carrier polymer with single-unit bonding strength Ti. During the low-energy ion beam deposition process, the current was 200A, the beam current was 700mA, and the deposition rate was 15nm / min; during the electron beam evaporation process, the power was 50kW, the deposition rate was 4μm / min, the roll-to-roll speed was 4m / min, the thickness of the copper foil was 1μm, and the surface roughness was 0.2μm, obtaining extremely thin and strippable copper.
[0065] Example 4
[0066] 1) The carrier polymer was sequentially cleaned by Penning ion source, Kaufman ion source and cold cathode Hall source roll-to-roll cleaning, wherein the voltage of Penning ion source cleaning was 20 kV, the time was 1 min, the oxygen flow rate was 25 sccm, the voltage of Kaufman ion source cleaning was 15 kV, the time was 3 min, the oxygen flow rate was 30 sccm, the voltage of cold cathode Hall source cleaning was 0.8 kV, the time was 5 min, the argon flow rate was 50 sccm, and the roughness of the carrier polymer after cleaning was 0.1 μm;
[0067] 2) Using a 10 keV high energy ion beam to implant Fe, Ni, Co, N and O elements into the carrier polymer (where the molar ratio of Fe, Ni, Co, N and O is 2:4:2:1:1), the implantation depth is 30 nm, and the implantation dose is 5×10 15 / cm 2, obtaining an ion implantation carrier polymer, the surface roughness of the ion implantation carrier polymer is 0.1 μm;
[0068] 3) using a low-energy ion beam to deposit unidirectional bonding strength metal Ti on the surface of the ion-implanted carrier polymer to obtain a carrier polymer with unidirectional bonding strength Ti, the deposition thickness of Ti is 100 nm, the porosity of the Ti film layer is 4%, and the roughness of the Ti film layer is 0.01 μm;
[0069] 4) Low-energy ion beam and electron beam evaporation were used to deposit extremely thin copper on the surface of a carrier polymer with single-unit bonding strength Ti. During the low-energy ion beam deposition process, the current was 120A, the beam current was 900mA, and the deposition rate was 13nm / min; during the electron beam evaporation process, the power was 60kW, the deposition rate was 4μm / min, the roll-to-roll speed was 4m / min, the thickness of the copper foil was 1μm, and the surface roughness was 0.05μm, obtaining extremely thin and strippable copper.
[0070] The present invention uses a 90° peeling test method to test the performance of the ultra-thin strippable copper prepared in Examples 1 to 4. The one-way bonding strength of the metal and the polymer, and the one-way bonding strength of the metal and the copper foil in the ultra-thin strippable copper are as follows: Figure 1 As shown, the porosity of the copper foil after deposition is as follows Figure 2 shown.
[0071] As can be seen from the above embodiments, the present invention provides a method for preparing ultra-thin strippable copper, which firstly plasma cleans the carrier polymer, then performs high-energy ion implantation on the cleaned carrier polymer, deposits a unidirectional bonding strength metal on the obtained ion-implanted carrier polymer, and finally deposits ultra-thin copper on the surface of the carrier polymer deposited with the unidirectional bonding strength metal, and finally obtains an ultra-thin strippable copper. Embodiments 1 and 2 of the present invention are ultra-thin strippable copper prepared without cleaning the carrier polymer and high-energy ion beam implantation, respectively. The bonding strength between the unidirectional bonding strength metal and the carrier polymer is very low, which is 0.14N / cm and 0.26N / cm respectively; with the increase of Ti thickness, the bonding strength between the unidirectional bonding strength metal and the carrier polymer increases slightly, and the bonding strength with the copper foil of Embodiments 1 to 4 remains basically unchanged. It can be seen that the ultra-thin strippable copper prepared by the present invention has a bonding strength between the unidirectional bonding strength metal and the carrier polymer of ≥0.7N / cm, and a bonding strength between the unidirectional bonding strength metal and the copper foil of 0.1 to 0.2N / cm. The porosity of Embodiments 1 and 2 is very high, which is 10% and 6% respectively. It can be seen that plasma cleaning has a significant effect on reducing porosity. The porosity of Examples 3 and 4 is below 5%, 4.8% and 2% respectively. With the increase of Ti thickness, the porosity decreases significantly, but considering the deposition speed and efficiency, the thickness of Ti should be selected preferentially.
[0072] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing ultra-thin strippable copper, characterized in that: The following steps are involved: 1) performing roll-to-roll plasma cleaning on the carrier polymer to obtain a cleaned carrier polymer; 2) performing high-energy ion implantation treatment on the cleaned carrier polymer to obtain an ion-implanted carrier polymer; The high energy ion implantation process is to implant elements using a high energy ion beam with an energy of 10 to 50 keV, with an implantation depth of 10 to 50 nm and an implantation dose of 1×10 15 ~1×10 16 / cm 2 , the surface roughness of the carrier polymer after injection is 0.01-0.1 μm; 3) depositing a one-way bonding strength metal on the ion-implanted carrier polymer to obtain a carrier polymer with one-way bonding strength metal deposited thereon; 4) depositing extremely thin copper on the surface of the carrier polymer with unidirectional bonding strength metal deposition to obtain extremely thin and strippable copper; The plasma cleaning in step 1) includes sequentially performing Penning ion source cleaning, Kaufman ion source cleaning, and cold cathode Hall source cleaning.
2. The method for preparing ultra-thin strippable copper according to claim 1, characterized in that: The voltage of the Penning ion source cleaning is 20-40 kV, the time is 1-5 min, and the oxygen flow rate is 10-50 sccm.
3. The method for preparing ultra-thin strippable copper according to claim 1, characterized in that: The voltage of the Kaufman ion source cleaning is 10-20 kV, the time is 1-5 min, and the oxygen flow rate is 10-50 sccm.
4. The method for preparing ultra-thin strippable copper according to claim 1, characterized in that: The voltage of the cold cathode Hall source cleaning is 0.5-1 kV, the time is 1-5 min, the argon gas flow rate is 10-50 sccm, and the roughness of the carrier polymer after cleaning is 0.1-0.4 μm.
5. The method for preparing ultra-thin strippable copper according to claim 1, characterized in that: The elements in step 2) include one or more of Fe, Ni, Co, N and O.
6. The method for preparing ultra-thin strippable copper according to any one of claims 2 to 4, characterized in that: In the step 3), a low-energy ion beam is used to deposit a unidirectional bonding strength metal, the deposition thickness is 10-100 nm, the porosity of the metal film layer is ≤5%, and the roughness of the metal film layer is 0.01-0.1 μm.
7. The method for preparing ultra-thin strippable copper according to claim 6, characterized in that: The unidirectional bonding strength metal in step 3) includes one or more of Ti, Zr and Mo.
8. The method for preparing ultra-thin strippable copper according to claim 7, characterized in that: In the step 4), low-energy ion beam and electron beam evaporation are used to deposit active thin copper. During the low-energy ion beam deposition process, the current is 90-200A, the beam current is >600mA, and the deposition rate is ≥10nm / min; during the electron beam evaporation process, the power is ≥30kW, the deposition rate is ≤5μm / min, and the roll-to-roll speed is ≥3m / min.