A color-developing etching solution and its preparation method and application

By adding inorganic, metallic elements and organic additives to the chromogenic corrosive solution on the basis of hydroxide, the problems of unclear color and short corrosion time of sodium hydroxide corrosive solution in welding penetration depth and width detection are solved. The color development is obvious and Clear, improving detection efficiency and accuracy.

CN116288357BActive Publication Date: 2024-10-11EVE POWER CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310283299.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-22
Publication Date
2024-10-11
Estimated Expiration
2043-03-22

AI Technical Summary

Technical Problem

The existing sodium hydroxide corrosive solution has problems such as unclear color, poor interface definition, easy erasure of corroded locations, and short storage time during lithium-ion battery welding penetration and width detection, resulting in low detection efficiency and accuracy.

Method used

A color-developing corrosive solution that combines hydroxide with inorganic, metallic elements and organic additives is used to develop color through precipitation reaction, increase color intensity and clarity, reduce corrosion time, and avoid corrosion to other parts of the sample.

Benefits of technology

The color development is more obvious and clear, and the color development time is shortened, which improves the efficiency and accuracy of welding penetration and width detection, avoids unnecessary corrosion of samples, and improves detection efficiency and accuracy.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116288357B_ABST
    Figure CN116288357B_ABST
Patent Text Reader

Abstract

The invention provides a color-developing etching solution and a preparation method and application thereof. The color-developing etching solution comprises a hydroxide and an additive, wherein the hydroxide comprises sodium hydroxide and / or potassium hydroxide; the additive comprises an inorganic additive, and the inorganic additive comprises a metal chloride and / or a metal sulfide; the color-developing etching solution takes less etching time, can avoid corrosion of other positions of a sample, and has obvious color development and high definition, thereby significantly reducing the detection time of the fusion depth and the fusion width, improving the detection efficiency, and can make the colors of the fusion depth and the fusion width more clearly visible, thereby improving the detection accuracy.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of color development, and relates to a color development etching solution and a preparation method and application thereof. Background Art

[0002] In the production of lithium-ion batteries, laser welding is required between the cover plate and the aluminum shell, and the penetration of the weld needs to be tested after welding. In order to detect the quality of laser welding and determine whether the laser welding meets the process standards, the most intuitive and important detection method is to test the penetration depth and width of the weld; and the full welding of the aluminum shell also requires the penetration depth and width of the welding position to be tested.

[0003] The conventional method for detecting the penetration depth and width of aluminum welding is: the weld is cut along the cross section, and metallographically polished, and then the polished metallographic section is immersed in a sodium hydroxide solution, and the chemical reaction between aluminum and sodium hydroxide is utilized, and the difference in the crystal structure of the metallographic structure at the welding position and the surrounding position is utilized. The difference in chemical energy between different crystal structures leads to thermodynamic and kinetic deviations in the reaction between aluminum metal and sodium hydroxide. At the same time, due to the existence of the galvanic cell reaction principle, the metallographic structure with high activity is sacrificed to protect the metallographic structure with low reactivity, so that there is a significant difference between the molten pool at the laser welding position and the surrounding welding materials, resulting in a significant difference in color and obvious interface stratification at the welding position. Under the observation and recording of an optical magnifying glass, the penetration depth and width of the aluminum welding position are obtained.

[0004] For example, CN 110057995A discloses a method for detecting the welding penetration of an aluminum shell of a lithium-ion battery, which comprises the following steps: 1) cutting a welding section after welding the aluminum shell and the cover plate; 2) grinding the welding section; 3) immersing the welding section in a 0.01-0.5 mol / L NaOH solution for 1-30 minutes; 4) measuring the welding penetration of the welding section after cleaning the welding section; The main problem with the detection of the welding penetration and width at the current welding point is whether the color at the corrosion position is clear, whether the interface is distinct, and whether it is convenient for subsequent observation and measurement; the current sodium hydroxide etching solution used for the above color development still has the following problems: ① the corrosion position is easy to be erased; ② the storage time is short; ③ the color development of the metallographic interface of the welding penetration and width is not obvious, etc.

[0005] At the same time, since the key parameters of the sodium hydroxide etching solution are: the concentration of the sodium hydroxide solution and the length of the etching time, in order to make the color of the welding position clearer, the existing technology increases the etching time and increases the concentration of the sodium hydroxide solution. However, increasing the etching time will reduce production efficiency, and increasing the sodium hydroxide concentration will cause corrosion to other positions of the aluminum shell, causing morphological damage to the test sample and excessive corrosion.

[0006] Based on the above research, it is necessary to provide a color-developing etching liquid that can improve the color intensity of the corrosion position, make the color clearer and more obvious, and at the same time, reduce the corrosion time and avoid the etching liquid from causing large-area corrosion to the sample, thereby improving the detection efficiency and accuracy of the melting depth and width. Summary of the invention

[0007] The object of the present invention is to provide a color-developing etching liquid and a preparation method and application thereof, and in particular to a color-developing etching liquid for detecting the welding depth and width of aluminum materials and a preparation method and application thereof. The color-developing etching liquid takes less etching time and can avoid corrosion to other positions of the sample. The color-developing etching liquid has obvious color and high clarity, thereby significantly reducing the detection time of the welding depth and width, improving the detection efficiency, and making the colors of the welding depth and width more clearly visible, thereby improving the detection accuracy.

[0008] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:

[0009] In a first aspect, the present invention provides a color-developing etching solution, the color-developing etching solution comprising a hydroxide and an additive, the hydroxide comprising sodium hydroxide and / or potassium hydroxide;

[0010] The additives include inorganic additives, and the inorganic additives include metal chlorides and / or metal sulfides.

[0011] The invention uses an alkaline hydroxide solution as a color-developing etching solution and additionally adds an additive. On the one hand, without increasing the concentration of the hydroxide solution and the etching time, the addition of the additive can make the color development more obvious and improve the color development intensity of the corrosion position; on the other hand, metal chloride and / or metal sulfide as the inorganic additive can cooperate with the hydroxide to react and generate metal hydroxide precipitation. The generated precipitation is adsorbed on the corrosion site of the welding position, thereby making the color development more obvious without damaging other positions.

[0012] Preferably, the additive further includes a metal element and / or an organic additive.

[0013] In order to further avoid the problem that the color at the corrosion position is easy to erase and the color development time is short, the present invention adds a metal element and / or an organic additive to the color development corrosion liquid. The strong adsorption effect of the metal element at the detection position not only avoids the above problems, but also further improves the color development intensity; the coordinated effect of the organic additive and the inorganic hydroxide solution makes the color development difficult to erase and increases the storage time of the color development corrosion liquid.

[0014] Preferably, the inorganic additive further comprises any one of hydrogen peroxide, ammonia water or sodium carbonate or a combination of at least two thereof. Typical but non-limiting combinations include a combination of hydrogen peroxide and ammonia water, or a combination of sodium carbonate and ammonia water.

[0015] The inorganic additives of the present invention also include hydrogen peroxide, ammonia water or sodium carbonate. The addition of hydrogen peroxide, ammonia water or sodium carbonate can promote the precipitation of metal chlorides, shorten the color development time, and promote the adsorption of precipitates.

[0016] When the inorganic additive of the present invention comprises two different components, the molar ratio between the different components is (1-3):(1-3); when the inorganic additive comprises three different components, the molar ratio between the different components is (1-3):(1-3):(1-3).

[0017] Preferably, the metal chloride comprises FeCl3 (ferric chloride) and / or CuCl2 (copper chloride).

[0018] Preferably, the metal element includes any one of Al, Fe or Cu, or a combination of at least two of them. Typical but non-limiting combinations include a combination of Al and Fe, or a combination of Fe and Cu.

[0019] When the metal element described in the present invention includes two different components, the molar ratio between the different components is (1-3):(1-3); when the metal element described in the present invention includes three different components, the molar ratio between the different components is (1-3):(1-3):(1-3).

[0020] Preferably, the organic additive comprises any one of a porphyrin reagent, a triphenylmethane alkaline reagent or a rhodamine reagent, or a combination of at least two of them. Typical but non-limiting combinations include a combination of a porphyrin reagent and a triphenylmethane alkaline reagent, or a combination of a rhodamine reagent and a triphenylmethane alkaline reagent.

[0021] Preferably, the porphyrin reagent includes any one of p-chlorophenylporphyrin, tetra-p-tolylporphyrin, 5,15-diphenylporphyrin, tetraphenylporphyrin copper or protoporphyrin, or a combination of at least two thereof.

[0022] Preferably, the triphenylmethane alkaline reagent includes triphenylmethane bromide and / or triphenylmethane chloride.

[0023] Preferably, the rhodamine reagent includes any one of rhodamine 6G, rhodamine B base, rhodamine chloride 110, dihydrorhodamine 123 or rhodamine 800, or a combination of at least two of them.

[0024] Preferably, in the color-developing etching solution, the mass fraction of the hydroxide is 1-10wt%, for example, it can be 1wt%, 3wt%, 5wt%, 7wt%, 9wt% or 10wt%, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0025] When the content of hydroxide in the color-developing etching solution of the present invention is within the above range, effective corrosion and color development can be achieved, thereby avoiding corrosion of other positions of the aluminum shell caused by excessively high hydroxide concentration.

[0026] Preferably, the additive is added in an amount of 1-20% of the amount of the hydroxide substance in the color-developing corrosion solution, for example, it can be 1%, 3%, 5%, 7%, 9%, 11%, 13%, 15%, 17%, 19% or 20%, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable, preferably 1-6%.

[0027] Preferably, the amount of the inorganic additive added is 1-5% of the amount of the hydroxide substance in the color-developing etching solution, for example, it can be 1%, 2%, 3%, 4% or 5%, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0028] If the proportion of the inorganic additives in the present invention is too high, a large number of side reactions will occur in the system, resulting in excessive consumption of sodium hydroxide. If the addition ratio is too low, the display effect is not obvious and the effect cannot be effectively exerted.

[0029] Preferably, the added amount of the metal element is less than 0.5% of the amount of hydroxide substance in the color-developing corrosion solution, but does not include 0.5%. For example, it can be 0.48%, 0.4%, 0.3%, 0.2% or 0.1%, but is not limited to the listed values. Other unlisted values ​​within the numerical range are also applicable.

[0030] If too much metal element is added, the color of the color developing solution will be too dark and adsorbed to the non-welding area, which will make it difficult to distinguish the depth and width of the weld. If too little metal element is added, the color developing effect will not be obvious.

[0031] Preferably, the amount of the organic additive added is less than 0.5% of the amount of the hydroxide substance in the color-developing etching solution, but does not include 0.5%. For example, it can be 0.48%, 0.4%, 0.3%, 0.2% or 0.1%, but is not limited to the listed values. Other unlisted values ​​within the numerical range are also applicable.

[0032] If too much organic additive is added, the color developing solution will be adsorbed in the non-welding area, resulting in unclear distinction of the melt depth and melt width. At the same time, too much organic color developing reagent will also increase the cost. If too little is added, the color developing effect will not be obvious.

[0033] The addition amount of the inorganic additive, the addition amount of the metal element and the addition amount of the organic additive as well as the total addition amount of the additives described in the present invention cooperate with each other to further improve the comprehensive color rendering performance.

[0034] In a second aspect, the present invention provides a method for preparing the color-developing etching solution as described in the first aspect, the preparation method comprising the following steps:

[0035] Mixing hydroxide, water and additives, and then standing and storing to obtain the color-developing etching solution;

[0036] The hydroxide includes sodium hydroxide and / or potassium hydroxide; the additive includes an inorganic additive, and the inorganic additive includes a metal chloride.

[0037] Preferably, the storage time is less than 15 days, for example, it can be 14 days, 10 days, 8 days, 6 days, 4 days, 2 days or 0 days, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0038] The color-developing etching liquid of the present invention can be prepared and used immediately, and can also be effectively stored for a period of time before use without affecting the color-developing effect, thereby avoiding the disadvantage of preparing and using the color-developing etching liquid immediately. However, after exceeding the above storage time, the color-developing effect is not good.

[0039] Preferably, the stirring rate of the mixing is 50-400 rpm, for example, 50 rpm, 100 rpm, 200 rpm, 300 rpm or 400 rpm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0040] Preferably, the standing time is 30-400 min, for example, 30 min, 100 min, 200 min, 300 min or 400 min, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0041] In a third aspect, the present invention provides an application of the color-developing etching liquid as described in the first aspect, wherein the application includes detection of the penetration depth and penetration width of aluminum welding.

[0042] Compared with the prior art, the present invention has the following beneficial effects:

[0043] The present invention solves the problems of reduced corrosion efficiency, damaged sample morphology and excessive corrosion caused by increasing the concentration of the etching solution and prolonging the etching time. By improving the components of the etching solution, the color intensity of the corrosion position is improved, making the color clearer and more obvious. At the same time, the etching time is reduced, and large-area corrosion of the sample by the etching solution is avoided, which is beneficial to improving the detection efficiency and detection accuracy of the melting depth and melting width. BRIEF DESCRIPTION OF THE DRAWINGS

[0044] Figure 1 This is a schematic diagram of the color development of the color developing etching solution described in Example 1 of the present invention;

[0045] Figure 2 This is a schematic diagram of the color development of the color developing etching solution described in Comparative Example 1 of the present invention. DETAILED DESCRIPTION

[0046] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0047] Example 1

[0048] This embodiment provides a color-developing etching solution, which includes sodium hydroxide and additives, and the additives include inorganic additives, metal elements and organic additives;

[0049] The inorganic additive includes FeCl3, CuCl2 and hydrogen peroxide in a molar ratio of 1:1:1;

[0050] The metal element comprises Cu and Fe in a molar ratio of 1:1;

[0051] The organic additive includes a porphyrin reagent, and the porphyrin reagent is p-chlorophenylporphyrin;

[0052] In the color-developing corrosion solution, the mass fraction of sodium hydroxide is 5wt%, the amount of the additive added is 3% of the amount of sodium hydroxide in the color-developing corrosion solution, the amount of the inorganic additive added is 2.5% of the amount of sodium hydroxide in the color-developing corrosion solution, the amount of the metal element added is 0.5% of the amount of sodium hydroxide in the color-developing corrosion solution, and the amount of the organic additive added is 0.5% of the amount of sodium hydroxide in the color-developing corrosion solution;

[0053] The preparation method of the color-developing etching solution comprises the following steps: mixing sodium hydroxide, water, inorganic additives, metal elements and organic additives according to the formula amount at a stirring rate of 300 rpm, stirring and standing for 200 minutes, and then storing for 6 days to obtain the color-developing etching solution;

[0054] The color development schematic diagram of the color developing etching solution is as follows Figure 1 shown.

[0055] Example 2

[0056] This embodiment provides a color-developing etching solution, which includes sodium hydroxide and additives, and the additives include inorganic additives, metal elements and organic additives;

[0057] The inorganic additives include FeCl3, CuCl2 and ammonia water in a molar ratio of 2:1:1;

[0058] The metal element comprises Al and Fe in a molar ratio of 2:1;

[0059] The organic additive comprises a triphenylmethane alkaline reagent, and the triphenylmethane alkaline reagent is triphenylmethane chloride;

[0060] In the color-developing corrosion solution, the mass fraction of sodium hydroxide is 1wt%, the amount of the additive added is 1.5% of the amount of sodium hydroxide in the color-developing corrosion solution, the amount of the inorganic additive added is 1% of the amount of sodium hydroxide in the color-developing corrosion solution, the amount of the metal element added is 0.2% of the amount of sodium hydroxide in the color-developing corrosion solution, and the amount of the organic additive added is 0.3% of the amount of sodium hydroxide in the color-developing corrosion solution;

[0061] The preparation method of the color-developing etching solution comprises the following steps: mixing sodium hydroxide solution, water, inorganic additives, metal elements and organic additives according to the formula amount at a stirring rate of 50 rpm, standing for 30 minutes after stirring, and then storing for 0 days to obtain the color-developing etching solution.

[0062] Example 3

[0063] This embodiment provides a color-developing etching solution, which includes sodium hydroxide and additives, and the additives include inorganic additives, metal elements and organic additives;

[0064] The inorganic additive includes FeCl3 and sodium carbonate in a molar ratio of 1:1;

[0065] The metal element includes Fe;

[0066] The organic additive includes a rhodamine reagent, and the rhodamine reagent is rhodamine 6G;

[0067] In the color-developing corrosion solution, the mass fraction of sodium hydroxide is 10wt%, the amount of the additive added is 5.9% of the amount of sodium hydroxide in the color-developing corrosion solution, the amount of the inorganic additive added is 5% of the amount of sodium hydroxide in the color-developing corrosion solution, the amount of the metal element added is 0.45% of the amount of sodium hydroxide in the color-developing corrosion solution, and the amount of the organic additive added is 0.45% of the amount of sodium hydroxide in the color-developing corrosion solution;

[0068] The preparation method of the color-developing etching solution comprises the following steps: mixing sodium hydroxide solution, water, inorganic additives, metal elements and organic additives according to the formula at a stirring rate of 400 rpm, stirring, standing for 400 minutes, and then storing for 14 days to obtain the color-developing etching solution.

[0069] Example 4

[0070] This embodiment provides a color-developing etching solution, which is the same as that of Embodiment 1 except that the inorganic additive does not include hydrogen peroxide and hydrogen peroxide is replaced by FeCl3 in equal moles.

[0071] Example 5

[0072] This embodiment provides a color-developing etching solution, which is the same as that of Embodiment 1 except that the color-developing etching solution does not contain a metal element.

[0073] Example 6

[0074] This embodiment provides a color-developing etching solution, which is the same as that of Embodiment 1 except that it does not contain an organic additive.

[0075] Example 7

[0076] This embodiment provides a color-developing etching solution, which is the same as that of Embodiment 1 except that the color-developing etching solution does not contain metal elements and organic additives.

[0077] Example 8

[0078] This embodiment provides a color-developing etching solution, which is the same as that of Embodiment 1 except that the amount of inorganic additives added is 7% of the amount of sodium hydroxide in the color-developing etching solution, so that the proportion of the total additives changes accordingly.

[0079] Example 9

[0080] This embodiment provides a color-developing etching solution, which is the same as that of Embodiment 1 except that the amount of inorganic additive added is 0.5% of the amount of sodium hydroxide in the color-developing etching solution, so that the proportion of the total additives changes accordingly.

[0081] Example 10

[0082] This embodiment provides a color-developing etching solution, which is the same as that of Embodiment 1 except that the amount of metal element added is 1% of the amount of sodium hydroxide in the color-developing etching solution, so that the proportion of the total additives changes accordingly.

[0083] Embodiment 11

[0084] This embodiment provides a color-developing etching solution, which is the same as that of Embodiment 1 except that the amount of organic additive added is 1% of the amount of sodium hydroxide in the color-developing etching solution, so that the proportion of the total additives changes accordingly.

[0085] Comparative Example 1

[0086] This comparative example provides a color-developing etching solution, wherein the color-developing etching solution is a sodium hydroxide solution with a mass fraction of 5wt%;

[0087] The color development schematic diagram of the color developing etching solution is as follows Figure 2 shown.

[0088] The color-developing etching liquid described in the above embodiments and comparative examples is used to corrode the aluminum shell, and the penetration depth and width of the aluminum shell welding position are detected, wherein the detection method comprises: (1) vertically cutting the welding position; (2) grinding the cut position, first grinding it with 150-mesh sandpaper, and then grinding it with 800-mesh fine sandpaper, and polishing the surface to make it smooth and flat; (3) immersing the polished position in the color-developing etching liquid; (4) placing the material after soaking and corrosion in clean water and soaking it for 20 seconds; (5) wiping off the water stains on the surface, and not wiping the soaked corrosion position; (6) placing it under a magnifying glass, three-dimensional, and two-dimensional to test the penetration depth and width; wherein, at the same color development degree, the time for the color-developing etching liquid described in the above embodiments and comparative examples to perform corrosion is shown in Table 1 below; at the same corrosion time, the color-developing etching liquid described in the above embodiments and comparative examples is used to perform corrosion, and the clarity of the penetration depth and width detected is shown in Table 1 below.

[0089] Table 1

[0090]

[0091]

[0092] From Table 1, we can see the following points:

[0093] The color-developing etching solution provided by the present invention has obvious color development, and the color development time is short at the same color development degree, which can shorten the color development time, improve the detection efficiency, and improve the detection accuracy of the melting depth and melting width; by combining Example 1 with Comparative Example 1, Figure 1 and Figure 2 By comparison, it can be seen that the present invention adds additional additives on the basis of the sodium hydroxide etching solution, which can significantly improve the color development effect, and the displayed color is clearer and more obvious; from Example 1 and Example 4, it can be seen that the additional addition of hydrogen peroxide and other substances to the inorganic additives can promote the precipitation of metal chlorides and further improve the color development efficiency; from Example 1 and Examples 5-7, it can be seen that the addition of metal single substances and organic additives can play a coordinated role between the components and further improve the color development effect; from Example 1 and Examples 8-9, it can be seen that too much or too little content of inorganic additives will affect the color development effect, and there is also the situation of causing too many side reactions; from Example 1 and Examples 10-11, it can be seen that the addition amount of metal single substances and organic additives should not be too high, otherwise it will affect the matching color development effect between the components.

[0094] In summary, the present invention provides a color-developing etching liquid and a preparation method and application thereof. The color-developing etching liquid takes less etching time and can avoid corrosion to other positions of the sample. The color development is obvious and the clarity is high, thereby significantly reducing the detection time of the melt depth and melt width, improving the detection efficiency, and making the color of the melt depth and melt width more clearly visible, thereby improving the detection accuracy.

[0095] The above description is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention are within the protection scope and disclosure scope of the present invention.

Claims

1. A color-developing etching solution, characterized in that: The color-developing etching solution comprises a hydroxide and an additive, wherein the hydroxide comprises sodium hydroxide and / or potassium hydroxide; The additives include: inorganic additives, metal elements and / or organic additives; The inorganic additive includes metal chloride and / or metal sulfide, and the metal chloride and / or metal sulfide reacts with hydroxide to form metal hydroxide precipitate; The organic additive includes any one of porphyrin reagents, triphenylmethane alkaline reagents or rhodamine reagents, or a combination of at least two of them.

2. The color developing etching solution according to claim 1, characterized in that: The inorganic additive further comprises any one of hydrogen peroxide, ammonia water or sodium carbonate or a combination of at least two thereof.

3. The color developing etching solution according to claim 1, characterized in that: The metal chloride includes FeCl3 and / or CuCl2.

4. The color developing etching solution according to claim 1, characterized in that: The metal element includes any one of Al, Fe or Cu, or a combination of at least two of them.

5. The color developing etching solution according to claim 1, characterized in that: The porphyrin reagent includes any one of p-chlorophenylporphyrin, tetra-p-tolylporphyrin, 5,15-diphenylporphyrin, tetraphenylporphyrin copper or protoporphyrin, or a combination of at least two thereof.

6. The color developing etching solution according to claim 1, characterized in that: The triphenylmethane alkaline reagent includes triphenylmethane bromide and / or triphenylmethane chloride.

7. The color developing etching solution according to claim 1, characterized in that: The rhodamine reagent includes any one of rhodamine 6G, rhodamine B base, rhodamine chloride 110, dihydrorhodamine 123 or rhodamine 800, or a combination of at least two of them.

8. The color developing etching solution according to claim 1, characterized in that: In the color-developing etching solution, the mass fraction of the hydroxide is 1-10wt%.

9. The color developing etching solution according to claim 1, characterized in that: The additive is added in an amount of 1-20% of the amount of the hydroxide substance in the color-developing etching solution.

10. The color-developing etching solution according to claim 9, characterized in that: The additive is added in an amount of 1-6% of the amount of the hydroxide substance in the color-developing etching solution.

11. The color-developing etching solution according to claim 1, characterized in that: The amount of the inorganic additive added is 1-5% of the amount of the hydroxide substance in the color-developing etching solution.

12. The color developing etching solution according to claim 1, characterized in that: The added amount of the metal element is less than 0.5% of the amount of the hydroxide substance in the color-developing etching solution, but excluding 0.5%.

13. The color-developing etching solution according to claim 1, characterized in that: The amount of the organic additive added is less than 0.5% of the amount of the hydroxide substance in the color-developing etching solution, but excluding 0.5%.

14. A method for preparing the color-developing etching solution according to any one of claims 1 to 13, characterized in that: The preparation method comprises the following steps: Mixing hydroxide, water and additives, and then standing and storing to obtain the color-developing etching solution; The hydroxide includes sodium hydroxide and / or potassium hydroxide; the additive includes an inorganic additive, and the inorganic additive includes metal chloride and / or metal sulfide.

15. The preparation method according to claim 14, characterized in that: The storage time is less than 15 days.

16. The preparation method according to claim 14, characterized in that: The stirring rate of the mixing is 50-400 rpm.

17. The preparation method according to claim 14, characterized in that: The standing time is 30-400 min.

18. A use of the color developing etching solution according to any one of claims 1 to 13, characterized in that: The applications include detecting the penetration depth and width of aluminum welds.