Metal paste for bonding and bonding method

By using 10-100nm metal nanoparticles and appropriate sintering aids in the bonding paste, the properties and sintering conditions of the paste are controlled, and the problems of poor end bonding and pores are solved, and high bonding strength for large-area joints are achieved. Uniformity, suitable for semiconductor devices in high temperature environments.

CN116325096BActive Publication Date: 2024-11-26DOWA ELECTRONICS MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080105648.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-09-30
Publication Date
2024-11-26
Estimated Expiration
2040-09-30

AI Technical Summary

Technical Problem

The prior art is prone to poor end bonding during large-area joints, resulting in pore formation, and may cause oxidation in high temperature environments, affecting bonding strength and durability.

Method used

Using a bonding paste containing 10-100nm metal nanoparticles, by controlling the composition and sintering conditions of the paste, ensuring that heat treatment is carried out at a specific heating rate in a nitrogen atmosphere, reducing pore formation, and appropriately adjusting the boiling point of the solvent at the calcining temperature or The decomposition temperature is formed to form a uniform metal bonding layer.

Benefits of technology

Even when the bonding area is large, the end pores can be reduced, and a bonding layer with high bonding strength and uniformity can be formed, thereby improving the reliability and durability of the semiconductor device.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116325096B_ABST
    Figure CN116325096B_ABST
Patent Text Reader

Abstract

The present invention provides a bonding paste capable of reducing the generation of voids at the end even when the bonding area is large and capable of forming a uniform bonding layer, and a bonding method using the same. Provided is a bonding metal paste comprising metal nanoparticles (A) having a primary particle size of 10 to 100 nm by number average, wherein when the paste is heated from 40°C to 700°C at a heating rate of 3°C / min in a nitrogen atmosphere, the cumulative weight loss value (L 700 ) is set as 100, the cumulative value of the weight loss when the temperature is increased from 40℃ to 100℃ (L 100 ) is less than 75, and the cumulative value of weight loss when the temperature is increased from 40℃ to 150℃ (L 150 ) is above 90, and the cumulative value of weight loss when the temperature is increased from 40℃ to 200℃ (L 200 ) is 98 or above.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a bonding material capable of forming a metal bonding layer having reduced voids at the end portion between the bonding material and a bonding method using the bonding material. Background Art

[0002] Conventionally, in semiconductor devices in which electronic components such as semiconductor chips are mounted on substrates such as copper substrates, the electronic components are fixed to the substrates using solder. However, in recent years, in consideration of the burden on the human body and the environment, the conventional lead-containing solder has been transitioned to lead-free solder.

[0003] In addition, in such semiconductor devices, electronic components are miniaturized in order to increase the mounting density on the substrate, so the current density that drives them tends to increase. As a result, the heat generated by the electronic components during operation will also increase. In addition, the technology of using SiC elements as semiconductor elements, which have lower losses and excellent characteristics compared to the widely used Si elements, is being studied. In semiconductor devices with such SiC elements mounted on the substrate, there are also cases where the operating temperature exceeds 200°C. In the manufacture of semiconductor devices that may be exposed to such high-temperature environments, it is necessary to use high-temperature solder with a high melting point as the solder to fix the electronic components to the substrate, but such high-temperature solder is difficult to make lead-free.

[0004] Under this trend, the present applicant has disclosed the following content so far: by including nanosilver particles in the paste and appropriately controlling its composition, it is possible to provide a bonding method that has high bonding strength even without using lead, which is an environmentally harmful substance, and is a low-temperature process and excellent in high-temperature durability. (Patent Documents 1 and 2)

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: Japanese Patent Application Publication No. 2015-004105

[0008] Patent Document 2: Japanese Patent Application Publication No. 2015-225842 Summary of the invention

[0009] Problem that the invention aims to solve

[0010] As a technology disclosed in Patent Documents 1 and 2, it is disclosed that the voids in the metal layer formed when the paste is applied and sintered can be reduced by using a combination of nano-sized silver particles and micro-sized silver particles and a sintering aid and a phosphate-based additive.

[0011] However, according to recent studies by the inventors, even a paste with an optimized structure may sometimes have poor bonding at the end, especially when a large area is bonded. If water or the like penetrates into the pores caused by the poor bonding at the end, it is estimated that there is a risk of slow oxidation of the portion, and therefore, it is strongly desired to have a paste structure that does not cause poor bonding even when the bonding area is large.

[0012] Therefore, an object of the present invention is to provide a bonding paste capable of reducing voids at the end portions even when the bonding area is large and forming a uniform bonding layer, and a bonding method using the same.

[0013] Solutions for solving problems

[0014] The present inventors conducted intensive studies to solve these problems and found that the above problems can be solved if not only the added components but also the properties of the paste formed after the addition are set to appropriate conditions for the paste, thereby completing the present invention.

[0015] That is, the first invention disclosed in the present specification is a metal paste for bonding, which contains at least metal nanoparticles (A) having a primary particle size of 10 to 100 nm in number average, and the cumulative value of weight loss when the paste is heated from 40°C to 700°C at a heating rate of 3°C / min in a nitrogen atmosphere (L 700 ) is set as 100, the cumulative value of the weight loss when the temperature is increased from 40℃ to 100℃ (L 100 ) is less than 75, and the cumulative value of weight loss when the temperature is increased from 40℃ to 150℃ (L 150 ) is above 90, and the cumulative value of weight loss when the temperature is increased from 40℃ to 200℃ (L 200 ) is 98 or above.

[0016] The second invention is a metal paste for bonding in which, in the first invention, the cumulative value of weight loss when the temperature is increased from 40° C. to 200° C. (L 200 ) is below 99.9.

[0017] The third invention is the following metal paste for joining: in the metal paste for joining described in the first or second invention, when the total amount of the metal paste for joining comprising metal particles containing metal nanoparticles (A), solvents, dispersants and other additives is set to 100 mass% and the calcination temperature is set to Tb (°C), the solvent having a boiling point or a decomposition temperature of greater than Tb-50 (°C) and less than Tb+50 (°C) is greater than 5 mass% and less than 10 mass%.

[0018] The fourth invention is the following metal paste for joining: in the metal paste for joining described in any one of the first to third inventions, when the total amount of the metal paste for joining comprising metal particles containing metal nanoparticles (A), solvents, dispersants and other additives is set to 100 mass% and the calcination temperature is set to Tb (°C), it contains less than 1.5 mass% of components with a boiling point or decomposition temperature higher than the calcination temperature Tb+50 (°C).

[0019] The fifth invention is a metal paste for bonding, comprising metal particles, wherein the metal particles at least comprise metal nanoparticles (A) having a primary particle size having a number average value of 10 to 100 nm, and the shrinkage rate of the metal particles contained in the paste measured in a thermomechanical analysis conducted while being pressurized at 0.1 MPa in a nitrogen atmosphere and heated from 30°C to 250°C at a heating rate of 3°C / min is less than 1.5%.

[0020] A sixth invention is the metal paste for joining according to the fifth invention, wherein the metal particles used have a shrinkage rate of 0.5% or less as measured by thermomechanical analysis performed while heating from 30°C to 200°C.

[0021] A seventh invention is the metal paste for joining according to the fifth or sixth invention, wherein the metal particles used have a shrinkage rate of 0.3% or less as measured by thermomechanical analysis performed while heating from 30°C to 175°C.

[0022] The eighth invention is the following metal paste for bonding: in any one of the first to seventh inventions, further comprising an average particle size (D 50 ) are metal particles (B) of 1.0 to 5.0 μm.

[0023] A ninth invention is the metal paste for bonding according to the eighth invention, wherein the weight mixing ratio of the metal nanoparticles (A) to the metal particles (B) is 0.25 or less in terms of (A) / (B).

[0024] The 10th invention is a method for joining two joined components, which comprises the following steps: a step of coating the metal paste for joining described in any one of the 1st to 9th inventions on the joined components; placing another joined component coated with the paste on the coating film on another joined component; and a step of raising the temperature to a sintering temperature of 200 to 350°C after placement and maintaining the temperature at the sintering temperature for no more than 2 hours to form a metal joining layer.

[0025] An eleventh invention is a bonding method according to the tenth invention, comprising a step of drying the bonding metal paste at a temperature of 50 to 150° C. after applying the bonding metal paste.

[0026] The twelfth invention is a bonding method according to the tenth or eleventh invention, wherein the rate of temperature increase from room temperature to the sintering temperature is 1.5 to 10° C. per minute.

[0027] The 13th invention is a bonding method as follows: In any one of the 10th to 12th inventions, the area (bonding area) to which the bonding metal paste is applied is 9 mm 2 above.

[0028] Effects of the Invention

[0029] According to the present invention, even when the bonding area is large, the occurrence of voids at the end can be reduced, a uniform bonding layer can be formed, and a bonded body with high bonding strength can be formed. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 It is a schematic diagram which shows the method of measuring the shear strength of a bonded body.

[0031] Figure 2 These are the results obtained by photographing the bonding portion formed using the bonding metal paste in Example 3 using a micro-focus X-ray transmission device.

[0032] Figure 3 These are the results of photographing the bonding portion formed using the bonding metal paste in Comparative Example 4 using a micro-focus X-ray transmission device. DETAILED DESCRIPTION

[0033] The metal paste for bonding and the bonding method of the present invention will be described.

[0034] <Metal paste for bonding>

[0035] Metal paste for bonding consists of specific metal particles, solvent, and additives to supplement properties.

[0036] [Metal Nanoparticles]

[0037] Regarding the metal nanoparticles used in the present invention, in addition to the metal nanoparticles that the applicant has already commercially available, as long as they meet the purpose of the invention of this application, commercially available particles and particles described in the literature can be used. As long as the method for making nanoparticles meets the particle size range and properties specified in the present invention, particles made by any method of wet method or dry method can be used. As metal nanoparticles that meet the purpose of the present invention, the average primary particle size (the number average particle size calculated from the transmission electron microscope photo and the scanning electron microscope photo) is 10 to 100nm, preferably 15 to 80nm, more preferably 20 to 60nm, and more preferably 20 to 40nm. The number average particle size is also referred to as the number average of the primary particle size. It is preferred that an organic coating (covering layer) for inhibiting natural sintering is formed on the surface of the particles. As the particle size becomes smaller, the melting temperature of the metal nanoparticles becomes lower, so the formation temperature of the joint body can be reduced, so it is preferred. However, in the case of being too small, a thick covering layer must be formed to avoid sintering at room temperature, so it is not preferred. If a thick coating is formed, it is easy to disperse the particles and obtain a monodisperse material, but it is not preferred because it requires high temperature treatment to remove the coating and promote the sintering of the metal, or organic matter will remain in the metal layer, which will cause the bonding strength to decrease and the conductivity to decrease. In addition, if it is too monodisperse, the particles become difficult to recover, which will also cause a decrease in productivity.

[0038] Regarding the covering layer, in order to form a high bonding strength, it is preferred to use a substance with low-temperature decomposition that can be removed at the formation temperature of the metal layer. If a substance with a large molecular weight is used, a calcination residue will remain in the sintered layer and is not preferred. Therefore, it is advisable to avoid polymers and high molecular substances. As an organic substance forming the covering layer, it is preferred to use a substance with a boiling point at least below the sintering temperature, and it is advisable to use a substance with a boiling point below 300°C, preferably below 250°C. As examples of the above-mentioned organic compounds, carboxylic acids, dicarboxylic acids, unsaturated fatty acids, or amines, thiols, and sulfides with a carbon number of less than 12 can be exemplified, and carboxylic acids, dicarboxylic acids, unsaturated fatty acids, and amines are particularly preferred. Specifically, octanoic acid, heptanoic acid, hexanoic acid, valeric acid, butyric acid, propionic acid, oxalic acid, malonic acid, ethylmalonic acid, succinic acid, methylsuccinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, sorbic acid, maleic acid, hexylamine, octylamine, etc. can be listed.

[0039] If the amount of organic matter covering the surface increases, the calcination temperature may become high, and impurities may remain in the calcined film, which is not suitable. The amount of organic matter covering the metal nanoparticles (powder) may be 0.1% by mass or more and 10% by mass or less, preferably 0.5% by mass or more and 5% by mass or less, and more preferably 1.0% by mass or more and 3.0% by mass or less.

[0040] In addition, it is preferred that the particles have a small shrinkage upon heating. Specifically, the shrinkage measured in a thermomechanical analysis performed while increasing the temperature from 30°C to 250°C at a rate of 3°C / minute under a nitrogen atmosphere at a pressure of 0.1 MPa is 1.5% or less, preferably 1.0% or less, and preferably 0.75% or less. The shrinkage measured in a thermomechanical analysis performed while increasing the temperature from 30°C to 200°C at a rate of 3°C per minute under a nitrogen atmosphere at a pressure of 0.1 MPa is preferably 0.5% or less. The shrinkage measured in a thermomechanical analysis performed while increasing the temperature from 30°C to 175°C at a rate of 3°C per minute under a nitrogen atmosphere at a pressure of 0.1 MPa is preferably 0.3% or less.

[0041] The metal used in the metal nanoparticles is not particularly limited as long as it can be used for the joining of components. Both precious metals and base metals can be used. As precious metals, for example, silver, gold, ruthenium, rhodium, palladium, iridium, platinum, etc. can be listed. If the ease of acquisition is taken into consideration, silver, gold, etc. can be appropriately used. If the cost is considered, silver is particularly preferred. As base metals, for example, copper, aluminum, iron, nickel, etc. can be listed. Here, the metal that can be used can be a single metal or an alloy.

[0042] [Metal particles]

[0043] In the present invention, when metal particles are used in combination, commercially available metal particles can be used. The particles in this case can be particles produced by a wet method or particles produced by a dry method. The metal particles used in the present invention include those having a cumulative 50% particle size (D ) converted by volume measured by a laser diffraction particle size distribution device. 50 The metal particles have a particle size of 1.0 to 5.0 μm. When the metal paste (coating film) is sintered, the metal nanoparticles are sintered to connect the metal particles to form a metal bonding layer. At this time, in order to prevent pores from forming in the metal bonding layer, the D 50 The particle size is preferably 1.2 to 3.0 μm, more preferably 1.4 to 2.0 μm.

[0044] The metal particles may also be covered with an organic compound in order to improve dispersibility, etc. In this case, it is preferred to cover the metal particles with an organic compound having a carbon number of 20 or less. Examples of such organic compounds include oleic acid and stearic acid. As for the amount of the covered organic matter, a small amount can suppress the adverse effects on the metal layer as in the case of metal nanoparticles, so it is preferred. Specifically, it can be 5.0% by mass or less, preferably 3.0% by mass or less.

[0045] In addition, it is preferred that the particles have a small shrinkage when heated, as described in the description of the metal nanoparticles, but in the case of using metal particles in combination, it is preferred that the metal nanoparticles and the metal particles have the same properties after mixing. Specifically, for a mixture of metal nanoparticles and metal particles, the shrinkage measured in a thermomechanical analysis performed while heating from 30°C to 250°C at a rate of 3°C per minute under a nitrogen atmosphere while pressurizing at 0.1MPa is 1.5% or less, preferably 1.0% or less, and more preferably 0.75% or less. The shrinkage measured in a thermomechanical analysis performed while heating from 30°C to 200°C at a rate of 3°C per minute under a nitrogen atmosphere while pressurizing at 0.1MPa is preferably 0.5% or less. The shrinkage measured in a thermomechanical analysis performed while heating from 30°C to 175°C at a rate of 3°C per minute under a nitrogen atmosphere while pressurizing at 0.1MPa is preferably 0.3% or less.

[0046] The metal used in the metal particles is not particularly limited as long as it can be used for the joining of components. Any of precious metals and base metals can be used. As precious metals, for example, silver, gold, ruthenium, rhodium, palladium, iridium, platinum, etc. can be listed. Considering the ease of acquisition, silver, gold, etc. can be appropriately used. Considering the cost, silver is particularly preferred. As base metals, for example, copper, aluminum, iron, nickel, etc. can be listed. Here, the metal that can be used can be a single metal or an alloy. Here, the same metal as the metal nanoparticles can be used, or other metals can be used.

[0047] When metal particles are added to the metal nanoparticles, the weight mixing ratio of the metal nanoparticles (A) to the metal particles (B) is preferably 0.25 or less in terms of (A) / (B). In addition, the proportion of the metal nanoparticles or the mixture of the metal nanoparticles and the metal particles in the metal paste for bonding is preferably 90% by mass or more.

[0048] [Solvent]

[0049] The solvent used in the present invention is preferably a solvent that has the property of volatilizing at a temperature lower than the calcination temperature. The volatilization may be evaporation based on boiling or decomposition. Specifically, it is preferred to use a solvent having a boiling point or decomposition temperature of 300°C or less.

[0050] The solvent used in the present invention may be a polar solvent or a non-polar solvent as long as it does not affect sintering, etc. However, if the compatibility with other components is taken into consideration, it is appropriate to select a polar solvent.

[0051] As the solvent used here, a plurality of solvents may be mixed and used for the purpose of adjusting the boiling point, viscosity, evaporation rate, etc. in the metal paste. As the solvent that can be mixed here, when the solvent is a polar solvent, the following solvents can be exemplified.Examples include water; terpineol, 3-hydroxy-2,2,4-trimethylpentyl isobutyrate (Texanol), phenoxypropanol, 1-octanol, 1-decanol, 1-dodecanol, 1-tetradecanol, Terusolve MTPH (manufactured by NIPPON TERPENE CHEMICALS, INC.), 2-[2-(4-methylcyclohexyl)propan-2-yloxy]ethanol (dihydroterpinyloxyethanol, manufactured by NIPPON TERPENE CHEMICALS, INC.), Terusolve TOE-100 (manufactured by NIPPON TERPENE CHEMICALS, INC.), Terusolve DTO-210 (manufactured by NIPPON TERPENE CHEMICALS, INC.), and Terusolve DTO-300 (manufactured by NIPPON TERPENE CHEMICALS, INC.). CHEMICALS, INC.) and other monohydric alcohols; 3-methyl-1,3-butanediol, 2-ethyl-1,3-hexanediol (octanediol), diethylene glycol hexyl ether, 2-ethyl hexanediol, diethylene glycol dibutyl ether, glycerol, dihydroxyterpineol, 3-methyl-1,2,3-butanetriol (isoprenetriol A (IPTL-A), NIPPON TERPENE CHEMICALS, INC.), 2-methyl-1,3,4-butanetriol (isoprenetriol B (IPTL-B), NIPPON TERPENE CHEMICALS, INC.) and other polyhydric alcohols; butyl carbitol, diethylene glycol monobutyl ether, pine oil methyl ether (NIPPON TERPENE CHEMICALS, INC.), dihydropine oil methyl ether (DIHYDROTERPINYL ETHER) (NIPPON TERPENE CHEMICALS, INC.) and other polyhydric alcohols. CHEMICALS, INC.) and other ether compounds; butyl carbitol acetate, diethylene glycol monobutyl ether acetate, ethylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether acetate, diethylene glycol monoethyl ether acetate and other ethylene glycol ether acetate; nitrogen-containing cyclic compounds such as 1-methylpyrrolidone and pyridine; γ-butyrolactone, methoxybutyl acetate, methoxypropyl acetate, ethyl lactate, 3-hydroxy-3-methylbutyl acetate, dihydroterpineol acetate, Terusolve IPG-2Ac (NIPPON TERPENE CHEMICALS, INC.), Terusolve THA-90 (NIPPON TERPENE CHEMICALS, INC.), Terusolve THA-70 (NIPPON TERPENE CHEMICALS, INC.) and other ester compounds; etc.

[0052] The inventors of the present invention have found that: when the boiling point (or decomposition temperature) is appropriately adjusted during the selection of the solvent mixture, the speed of forming the metal layer can be adjusted and the metal layer can be appropriately formed. Specifically, by mixing a plurality of solvents with different boiling points and setting the cumulative value of the weight loss at each stage of calcination measured in a nitrogen atmosphere to a specific range, it is possible to avoid the solvent or additives generated during calcination, and the gas components generated during the volatilization or decomposition of organic matter constituting the surface of the metal particles remaining in an amount greater than the required amount.

[0053] [Solvents with different boiling points]

[0054] In the present invention, it is important to classify the boiling points of the solvents in the above-mentioned solvent candidates into layers, and by combining them, the boiling and decomposition of the solvents are not performed all at once but in multiple stages during the formation of the metal layer. By doing so, it is possible to alleviate the situation where the shrinkage of the metal layer caused by sintering is excessive all at once.

[0055] According to the inventors' research, if the composition of the paste of the present invention is roughly divided, when the boiling point or decomposition temperature (the desired sintering temperature: Tb) is set as the central value, a solvent (S) containing a boiling point or decomposition point of (the desired sintering temperature) ± 50°C is used. A ) and (desired sintering temperature: Tb) + 50°C or higher solvent or poorly decomposable organic matter (including those included in the category of solvent in Table 1 below, also collectively referred to as component S B ) is suitable, and it is confirmed that when (the desired sintering temperature) is set as the central value, a solvent (S) having a boiling point or a decomposition point of (the desired sintering temperature: Tb) ± 50°C A ) in the entire paste in a ratio of 5 mass % or more and 10 mass % or less, and a component (S) having a boiling point or a decomposition temperature higher than (desired sintering temperature: Tb) + 50°C B ) is more than 0 mass % and less than 1.5 mass %. As a specific example, when the calcination temperature (Tb) is set to 250°C (Examples and Comparative Examples described later), S A The range is 200-300°C, which means that the formula of the paste is determined by the components with a boiling point or decomposition temperature of 200°C or more and 300°C or less and the components above 300°C. In other words, in the present invention, the presence of organic matter with a high boiling point or carbon derived from organic matter is allowed in the metal layer. It is speculated that the presence of the organic matter with a high boiling point has the effect of inhibiting the excessive sintering of the metal component after the surface covering is detached during sintering. However, if there are too many such substances, the sintering of the particles will be hindered, which will have an adverse effect on the bonding strength, and therefore, it is not suitable.

[0056] As a specific example, the solvent formulation when the baking temperature is set to 250°C is described. When the baking temperature (Tb) is set to 250°C, the boundary temperature of the boiling point or decomposition temperature is 300°C, and as the composition of the solvent, a solvent with a boiling point or decomposition temperature of 200 to 300°C and a solvent with a temperature higher than 300°C are mixed. At this time, the solvent with a boiling point or decomposition temperature of 200 to 300°C (S A ), 1-decanol (boiling point (nominal value): 233°C), 3-methyl-1,2,3-butanetriol (isoprenetriol A (IPTL-A)) (boiling point (nominal value): 255°C, manufactured by NIPPON TERPENE CHEMICALS, INC.), 2-methyl-1,3,4-butanetriol (isoprenetriol B (IPTL-B)) (boiling point (nominal value): 278°C, manufactured by NIPPON TERPENE CHEMICALS, INC.) and diethylene glycol (boiling point (nominal value): 245°C). Here, it is presumed that when (temperature desired for sintering: Tb) is set as the central value, a solvent having a boiling point or a decomposition point of (temperature desired for sintering: Tb) ±50°C will play a role in quickly removing organic matter for protecting the surface from the particles, especially in the initial stage of forming the bonding layer. Since the boiling point or decomposition point is also low, it is necessary to mix a large amount in the solvent constituting the paste, and it is suitable to use at least 5% by mass and 10% by mass of the total mass. Since the viscosity of this solvent is also small, if the amount is increased excessively, it will become ink-like, which makes it difficult to apply it into the target shape, so it is not suitable. According to the opinions of the inventors, in order to optimize the fine pores after coating and baking, when the baking temperature is set to Tb (℃), it is preferred to make the boiling point or decomposition temperature in the region above Tb-50 (℃) and below Tb+50 (℃). If a specific example is given, when the baking temperature is 250℃, when a substance with a boiling point or decomposition temperature of 250℃ to 300℃ is added, it is possible to show a good balance between bonding strength and fine pores, so it is preferred. When the total amount of the metal paste for bonding containing metal particles containing metal nanoparticles, solvents, dispersants and other additives is set to 100 mass% and the baking temperature is set to Tb (°C), the solvent having a boiling point or decomposition temperature of Tb-50 (°C) or more and Tb+50 (°C) or less is preferably 5 mass% or more and 10 mass% or less. It is preferred that the component having a boiling point or decomposition temperature higher than the baking temperature Tb+50 (°C) is contained in an amount of more than 0 mass% and less than 1.5 mass%. The baking temperature Tb can be set to a value within the range of 200 to 300°C.

[0057] When the calcination temperature (Tb) is set to 250°C, the solvent (S) having a boiling point or a decomposition temperature higher than 300°C (Tb+50°C) is used. B) include solvents such as Terusolve MTPH (boiling point (nominal value): 308-318°C, manufactured by NIPPONTERPENE CHEMICALS, INC.) and SOLPLUSD540 (boiling point: 700°C). Regarding the boiling point or decomposition temperature mentioned here, in addition to the values ​​recorded in the manufacturer's SDS, etc., you can also use the values ​​calculated by TG / DTA, etc. At this time, the measurement start temperature is set to 25°C and the temperature is increased from 25°C at a rate of 3°C / min, and the temperature at which the thermal weight loss reaches 95% is taken as the boiling point of the substance. In the case where the thermal weight loss is less than 95% even if the temperature is increased to 700°C, for convenience, the boiling point of the substance is regarded as 700°C.

[0058] If there is too much of the above-mentioned substances, it will hinder the sintering of the particles and have an adverse effect on the bonding strength, so it is not suitable. If a solvent with a boiling point or decomposition temperature exceeding 300°C (calcination temperature 250°C + 50°C) is added in an amount greater than the required amount, it will hinder the calcination and there is a concern that unsintered parts will be produced, so care should be taken. According to the opinions of the inventors, it is appropriate for such a solvent to exceed 0% by mass and be less than 2.5% by mass, preferably less than 1.5% by mass, more preferably less than 1.0% by mass, and more preferably less than 0.5% by mass. Regarding the ratio of the amount of solvent with a temperature higher than 300°C (calcination temperature 250°C + 50°C) to the amount of solvent below 300°C (calcination temperature 250°C + 50°C), it is preferred to use 1 part of solvent with a temperature higher than 300°C (calcination temperature 250°C + 50°C) and more than 9 parts of solvent below 300°C (calcination temperature 250°C + 50°C) (the composition of the solvent with a temperature higher than (calcination temperature 250°C + 50°C) is less than 10% of the entire solvent).

[0059] The content of the solvent having a boiling point or decomposition temperature of 230°C or more and 300°C or less in the aforementioned bonding material is preferably an amount that accounts for 50% or more of the mass of all solvents in the aforementioned bonding material. The content of the solvent having a boiling point or decomposition temperature exceeding 300°C in the aforementioned bonding material is preferably an amount that accounts for 35% or less of the mass of all solvents in the aforementioned bonding material. The lower limit is preferably 2%, and more preferably 3%. The content of the solvent having a boiling point or decomposition temperature of 400°C or more in the aforementioned bonding material is preferably an amount that accounts for 6% or less of the mass of all solvents in the aforementioned bonding material. The lower limit is preferably 3%. It is preferred to satisfy any of the above content regulations, and it is more preferred to satisfy the regulations for all contents.

[0060] [The cumulative value of weight loss at 700°C L 700 ]

[0061] The weight loss of the metal paste at 40 to 700°C is the sum of the solvents, additives and organic matter constituting the surface of the particles constituting the paste. The reason for using the weight loss after heat treatment at a high temperature much higher than the heat treatment temperature of the paste of the present invention (maximum 300°C) as a reference is that the amount of organic matter that can be removed in the paste is calculated by using the temperature at which the flame retardant or difficult to decompose substances in the paste can be removed as a reference. If the temperature is set to a higher temperature than this, the sintering of the metal proceeds, and the organic matter is captured in the metal layer and becomes incapable of functioning, so it is not suitable. Hereinafter, the weight loss will also be referred to as the weight loss value.

[0062] Regarding weight loss, for example, there are the following calculation methods: prepare a paste, fully heat it at 40°C and then measure the weight, set the internal temperature to 700°C, place it in an electric furnace replaced with nitrogen, fully heat it, take it out of the furnace, and then measure the weight again, and calculate it from the weight loss before and after the heat treatment at 700°C; the method of calculating using a commercially available TG / DTA device, the latter can not only obtain the desired heating rate, but also calculate the reduction at 100°C and the reduction at 150°C at one time, so it is suitable. As an example of the measurement method using a TG / DTA device, the following method can be cited: using a TG / DTA (TG / DTA6300) manufactured by SII, 10±1 mmg of the bonding material is weighed in an alumina pan (φ0.5 mm) for measurement, and the temperature is increased from 40°C to 700°C at a heating rate of 3°C / min in a nitrogen atmosphere of 200 mL / min, and the calculation is performed.

[0063] [The cumulative value of weight loss at 100°C L 100 ]

[0064] The weight loss of the metal paste of the present invention at 40 to 100° C. in nitrogen is calculated by calculating the cumulative weight loss value L at 40 to 700° C. 700 When it is set to 100, it is more than 25 and less than 75, preferably more than 30 and less than 70, more preferably less than 60, and more preferably less than 50. If this value shows a value greater than 70, it means that the solvent is separated from the paste at once in the low temperature region, and therefore it also becomes the cause of uneven sintering, so it is not preferred. In addition, by making a certain amount of non-metallic components such as solvents remain, the reduction of the contact points of the metal nanoparticles and the joined components caused by the opposite behavior of the thermal expansion of the joined components brought by the temperature increase and the shrinkage of the coating formed by the joining material can be suppressed, thus contributing to the good formation of the metal layer, so it is preferred.

[0065] [The cumulative value of weight loss at 150°C L 150 ]

[0066] The weight loss of the metal paste of the present invention at 40 to 150° C. in nitrogen is calculated by accumulating the weight loss at 40 to 700° C. 700 When the value is 100, it is 90 or more, preferably 93 or more, and more preferably 95 or more. If the value is low, the paste contains many components that are difficult to decompose and difficult to release, which may affect the formation of the metal layer, which is not preferred.

[0067] [The cumulative value of weight loss at 200°C L 200 ]

[0068] The weight loss of the metal paste of the present invention at 40 to 200° C. in nitrogen is calculated by accumulating the weight loss at 40 to 700° C. 700 When the value is set to 100, it is 95 or more, preferably 98 or more. When the value is low, there are many components that are difficult to decompose and difficult to separate in the paste, which may affect the formation of the metal layer, so it is not preferred. If the value exceeds 99.9, when the baking temperature is set to 200 to 300°C, the sintering of the particles may sometimes proceed locally, which is not preferred.

[0069] [Other added substances]

[0070] Known additives may be added to the paste of the present invention in a suitable range within the range that does not affect the sinterability and bonding strength of the paste. Specifically, dispersants such as acid dispersants and phosphate dispersants, sintering promoters such as glass powder, antioxidants, viscosity modifiers, organic binders (such as resin binders), inorganic binders, pH adjusters, buffers, defoamers, leveling agents, and volatilization inhibitors can be listed. The content of the additives in the bonding material is preferably 0.1% by mass or less.

[0071] <Method for producing metal paste>

[0072] The metal paste of the present invention can be produced by kneading metal nanoparticles and a solvent and any other components by a known method. The kneading method is not particularly limited, and for example, each component is prepared separately and kneaded in any order by using an ultrasonic disperser, a bulk material machine, a three-roll mill, a ball mill, a bead mill, a twin-screw kneader or a revolving mixer, etc., thereby producing a metal paste for bonding.

[0073] <Joining method>

[0074] The joining based on the present invention is a method of joining two joined components using an embodiment of the joining material of the present invention. By using this method, a uniform joining layer can be formed until the end, and a joined body with high joining strength and a sufficiently reduced porosity of the metal joining layer can be obtained. The embodiment of the joining method of the present invention has a coating film forming process, a loading process and a sintering process, and other pre-drying processes can also be implemented. These processes are described below.

[0075] [Coating film forming step]

[0076] In this process, the metal paste for bonding of the present invention is applied to a bonded member by a printing method such as screen printing, metal mask printing, inkjet printing, etc. to form a coating film. The selected printing method can be used to appropriately adjust the viscosity of the paste and ink. As an example of the aforementioned bonded member, a substrate can be cited. As a substrate, a metal substrate such as a copper substrate, an alloy substrate of copper and a certain metal (such as W (tungsten), Mo (molybdenum)), a ceramic substrate in which a copper plate is clamped between SiN (silicon nitride), AlN (aluminum nitride), etc., and then a plastic substrate such as a PET (polyethylene terephthalate) substrate, a printed circuit substrate according to the situation, etc. can be cited. Furthermore, the laminated substrate formed by stacking them can also be applied to the bonding method of the present invention. The position of the bonded member to be coated with the bonding material can also be plated with metal. From the viewpoint of bonding compatibility with the metal component in the coating film, the type of metal in the metal plating of the aforementioned bonded member can also be the same as the constituent metal of the metal component in the bonding material.

[0077] [Placing process]

[0078] Next, another member to be joined is placed on the coating film formed on the aforementioned one member to be joined. Examples of the other member to be joined include semiconductor elements such as Si chips and SiC chips, and substrates that are the same as the members listed as an example of a member to be joined. In addition, the paste may be applied to the back of a Si chip, SiC chip, or IC chip instead of the substrate.

[0079] In addition, the position (joined surface) to be in contact with the coating of another joined component can also be plated with metal. From the viewpoint of bonding compatibility with the metal component in the coating, the type of metal in the metal plating of the aforementioned other joined component is preferably the same as the constituent metal of the metal component in the bonding material. In addition, when the joined component is placed on the coating, external pressure in the direction of compressing the coating in addition to the deadweight of the joined object can also be applied between the two joined components, but it is important to use a pressure to the extent that the chip, substrate, etc. will not be damaged by the external pressure.

[0080] In addition, the bonding method of the present invention can be used to bond large-area semiconductor elements. In particular, when the bonding surface of the semiconductor element (the surface in contact with the coating or the metal bonding layer formed therefrom. The coating is usually formed in a manner that covers the entire bottom surface of the semiconductor element) is 9 mm 2 In the above case, the embodiment of the joining method of the present invention is suitable, and the area of ​​the joined surface is 25mm 2 The above situation is more suitable when the area of ​​the joint surface is 36 to 400 mm 2 It is particularly suitable for the case.

[0081] [Pre-drying process]

[0082] When the coating film carried by another joined member is heated and sintered, in order to remove the excess organic components, a pre-drying process for pre-drying the coating film can be implemented before or after another joined member is placed on the coating film (before or after the placing process). The purpose of pre-drying is to remove a portion of the solvent from the coating film, and to dry it under the condition that the solvent is volatilized and the metal nanoparticles are substantially not sintered. Therefore, pre-drying is preferably implemented by heating the coating film at 60 to 150 ° C. The drying based on the heating can be carried out at atmospheric pressure or under reduced pressure to vacuum. In addition, in the sintering process described below, if the heating rate to the sintering temperature is less than 7 ° C / minute, the pre-drying process can be implemented by heating to the sintering temperature. When the components of the substrate and the metal particles contain easily oxidized metals as constituent components (for example, assuming that copper and copper alloys are used as the metal and metal particles of the substrate), it is preferably implemented in an inert atmosphere from the viewpoint of preventing oxidation.

[0083] [Sintering process]

[0084] After the placement process and the pre-drying process as needed, the coating film sandwiched between the two joined members is heated from room temperature to a sintering temperature of 200 to 350°C at a heating rate of 1.5°C / min to 10°C / min, and the sintering temperature is maintained for more than 1 minute and less than 2 hours to form a metal bonding layer from the coating film. The metal bonding layer has excellent bonding strength and few pores. Therefore, through this sintering, the two joined members can be firmly bonded with high reliability.

[0085] The heating rate when heating to the sintering temperature in the sintering process is preferably 2°C / min to 6°C / min, and more preferably 2.5°C / min to 4°C / min, from the viewpoint of forming a bonded body having a metal bonding layer with high bonding strength and few pores. In addition, if such a heating rate is used, the heating to the sintering temperature can also serve as a pre-drying process.

[0086] From the viewpoint of the bonding strength and cost of the metal bonding layer to be formed, the sintering temperature is preferably 220 to 300°C. From the viewpoint of the bonding strength and cost of the metal bonding layer to be formed, the time of holding the sintering temperature is preferably 1 to 90 minutes. In addition, during the heating to the sintering temperature and the holding at the sintering temperature, it is not necessary to apply pressure in the direction of compressing the coating film between the joined members, but for the purpose of forming a denser sintered film, a pressure of 5 MPa or less may be applied.

[0087] In addition, the sintering process can be carried out in an air atmosphere or in an inactive atmosphere such as a nitrogen atmosphere. However, particularly when the components of the substrate and the metal particles contain easily oxidized metals as constituent components (for example, assuming that copper or a copper alloy is used as the metal of the substrate and the metal particles), from the perspective of preventing oxidation, it is preferably carried out in an inactive atmosphere, and from the perspective of cost, it is more preferably carried out in a nitrogen atmosphere.

[0088] The metal layer formed after sintering becomes a dense metal layer in which pores are not recognizable from a macroscopic perspective, but pores with extremely small diameters can be confirmed from the X-ray transmission image. It is generally believed that it is preferable to have as few pores as possible, but for the paste of the present invention, high bonding strength can be obtained when pores with small particle sizes exist to a certain extent. Nevertheless, when there are too many pores, it may have an adverse effect on the fatigue life of the joint, so it is not preferred. The pore occupancy ratio calculated from the X-ray transmission image can be less than 10%, preferably less than 5%, and more preferably less than 3%.

[0089] Example

[0090] The present invention will be described in more detail below using Examples and Comparative Examples, but the present invention is not limited thereto.

[0091] <Preparation of Metal Paste for Joining (Examples 1 to 5, Comparative Examples 1 to 7)>

[0092] [Preparation of Metal Nanoparticles]

[0093] 3400 g of water was placed in a 5 L reaction tank, and nitrogen was flowed into the water in the reaction tank at a flow rate of 3000 mL / min for 600 seconds from a nozzle provided at the bottom of the reaction tank. After removing dissolved oxygen, nitrogen was supplied to the reaction tank at a flow rate of 3000 mL / min from the top of the reaction tank, and a nitrogen atmosphere was formed in the reaction tank. While stirring with a stirring rod with a stirring blade provided in the reaction tank, the temperature of the water in the reaction tank was adjusted to 60°C. 7 g of ammonia water containing 28% by mass of ammonia was added to the water in the reaction tank, and stirred for 1 minute to prepare a uniform solution. 45.5 g of hexanoic acid (manufactured by Wako Pure Chemical Industries, Ltd.), a saturated fatty acid as an organic compound, was added to the solution in the reaction tank (molar ratio relative to silver was 1.98), and after stirring for 4 minutes to dissolve, 23.9 g of 50% by mass of hydrazine hydrate (manufactured by Otsuka Chemical Co., Ltd.) as a reducing agent (4.82 equivalents relative to silver) was added to prepare a reducing agent solution.

[0094] In addition, a silver nitrate aqueous solution obtained by dissolving 33.8 g of silver nitrate crystals (manufactured by Wako Pure Chemical Industries, Ltd.) in 180 g of water was prepared as a silver salt aqueous solution, the temperature of the silver salt aqueous solution was adjusted to 60° C., and 0.00008 g of copper nitrate trihydrate (manufactured by Wako Pure Chemical Industries, Ltd.) was added to the silver salt aqueous solution (1 ppm in terms of copper relative to silver). It should be noted that the addition of copper nitrate trihydrate was performed by adding an aqueous solution obtained by diluting a copper nitrate trihydrate aqueous solution having a certain high concentration so as to achieve a target copper addition amount.

[0095] Next, the above-mentioned silver salt aqueous solution is added to the above-mentioned reducing agent solution at one time for mixing, and the reduction reaction is started while stirring. About 10 seconds after the reduction reaction starts, the color change of the slurry as the reaction solution ends. After aging for 10 minutes while stirring, the stirring is terminated, and solid-liquid separation based on suction is performed. The solid obtained is washed with pure water and vacuum dried at 40°C for 12 hours to obtain a dry powder of silver nanoparticles (covered with caproic acid). It should be noted that the proportion of silver in the silver nanoparticles is calculated to be 97% by mass by weight after removing caproic acid by heating. In addition, the average primary particle size of the silver nanoparticles was obtained by transmission electron microscopy (TEM), and the result was 17nm.

[0096] [Metal particles]

[0097] As metal particles, silver particles AG-3-60 (manufactured by DOWAHIGHTECH CO., LTD.) having an average primary particle diameter of 800 nm as measured by a scanning electron microscope were prepared.

[0098] [Preparation of metal paste for bonding]

[0099] The metal components and non-metal components described in the following Table 1 were kneaded at the blending ratios (mass %) described in Table 1 to prepare bonding materials of Examples 1 to 5 and Comparative Examples 1 to 7. In Table 1, the non-metal component is referred to as a solvent.

[0100] [Preparation of a joint body for evaluation of joint strength and voids]

[0101] The bonding materials of Examples 1 to 5 and Comparative Examples 1 to 7 prepared above were coated on a 10 mm × 10 mm (1 mm thick) copper substrate using a metal mask (opening 2.5 mm × 2.5 mm, thickness 70 μm). A 2 mm × 2 mm (0.3 mm thick) Si element with a square bottom (bonded surface) was placed on the coating film of each bonding material formed on the copper substrate, and a force of 0.47 N was applied for 1 second. The temperature was raised from 25°C to 250°C at 3°C / min in a N2 atmosphere, and baked at 250°C for 60 minutes to form a silver bonding layer to obtain a bonded body.

[0102] [Evaluation of shear strength of bonded body]

[0103] Use SERIES4000 (made by DAGE), such as Figure 1 As shown, the shear strength of the bonded body obtained above was measured. Specifically, the bonded body includes: a copper substrate 3, a silver bonding layer 2 formed thereon, and a Si element 1 formed thereon and bonded to the copper substrate 3 through the silver bonding layer 2. From the side of the Si element 1, a force is applied with a shearing tool 4 in the horizontal direction of the copper substrate 3 at a setting of 5 mm / min, and the force at the time of fracture is divided by the area of ​​the bottom surface of the Si element 1 to obtain the shear strength of the bonded body. It should be noted that the above test is carried out in a manner that the lower end of the shearing tool 4 is in contact with a position 50 μm in height from the copper substrate 3.

[0104] [Pore Evaluation]

[0105] The bonding portion of each bonded body, Si element-silver bonding layer-copper substrate, was photographed using a micro-focus X-ray fluoroscopy device (SMX-16LT, manufactured by Shimadzu Corporation), and the obtained image was binarized using image processing software (trade name: PaintShop). Figure 2 These are the results of photographing the bonding portion formed using the bonding metal paste in Example 3 using a microfocus X-ray transmission device. Figure 3 The results are obtained by photographing the bonded portion formed using the bonding metal paste in Comparative Example 4 using a microfocus X-ray transmission device. Then, the porosity was determined. The shear strength and porosity of the obtained particles are shown in Table 1.

[0106] [Table 1]

[0107]

[0108] <Preparation of Metal Paste for Joining (Example 6 and Comparative Example 8)>

[0109] (Preparation of Metal Nanoparticles)

[0110] 3400 g of water was placed in a 5 L reaction tank, and nitrogen was flowed into the water in the reaction tank at a flow rate of 3000 mL / min for 600 seconds from a nozzle provided at the bottom of the reaction tank. After removing dissolved oxygen, nitrogen was supplied to the reaction tank at a flow rate of 3000 mL / min from the top of the reaction tank, and a nitrogen atmosphere was formed in the reaction tank. While stirring with a stirring rod with a stirring blade provided in the reaction tank, the temperature of the water in the reaction tank was adjusted to 60°C. 7 g of ammonia water containing 28% by mass of ammonia was added to the water in the reaction tank, and stirred for 1 minute to prepare a uniform solution. 45.5 g of hexanoic acid (manufactured by Wako Pure Chemical Industries, Ltd.), a saturated fatty acid as an organic compound, was added to the solution in the reaction tank (molar ratio relative to silver was 1.98), and after stirring for 4 minutes to dissolve, 23.9 g of 50% by mass of hydrazine hydrate (manufactured by Otsuka Chemical Co., Ltd.) as a reducing agent (4.82 equivalents relative to silver) was added to prepare a reducing agent solution.

[0111] In addition, a silver nitrate aqueous solution obtained by dissolving 33.8 g of silver nitrate crystals (manufactured by Wako Pure Chemical Industries, Ltd.) in 180 g of water was prepared as a silver salt aqueous solution, the temperature of the silver salt aqueous solution was adjusted to 60° C., and 0.00008 g of copper nitrate trihydrate (manufactured by Wako Pure Chemical Industries, Ltd.) was added to the silver salt aqueous solution (1 ppm in terms of copper relative to silver). It should be noted that the addition of copper nitrate trihydrate was performed by adding an aqueous solution obtained by diluting a copper nitrate trihydrate aqueous solution having a certain high concentration so as to achieve a target copper addition amount.

[0112] Next, the above-mentioned silver salt aqueous solution is added to the above-mentioned reducing agent solution at one time for mixing, and the reduction reaction is started while stirring. About 10 seconds after the reduction reaction starts, the color change of the slurry as the reaction solution ends, and after aging for 10 minutes while stirring, the stirring is terminated, and solid-liquid separation based on suction is performed, and the solid obtained is washed with pure water, and vacuum dried at 40°C for 12 hours to obtain a dry powder of silver particles (covered with caproic acid). It should be noted that the proportion of silver in the silver particles is calculated to be 97% by mass by weight after removing caproic acid by heating. In addition, the average primary particle size of the silver particles is obtained by transmission electron microscopy (TEM), and the result is 17nm.

[0113] [Metal particles]

[0114] As metal particles, silver particles AG-3-60 (manufactured by DOWAHIGHTECH CO., LTD.) having an average primary particle size of 800 nm as determined by a scanning electron microscope photograph (SEM image) were prepared. In addition, for comparison, AG-2-1C (manufactured by DOWAHIGHTECH CO., LTD.) having an average primary particle size of 300 nm as determined by a scanning electron microscope photograph (SEM image) was prepared.

[0115] [Preparation of metal paste for bonding]

[0116] The silver particles and solvent described in the following Table 1 and other components were kneaded at the blending ratios (mass %) described in Table 1 to prepare bonding materials of Example 1 and Comparative Example 1.

[0117] [Thermomechanical analysis of metal particles]

[0118] Silver particles and AG-3-60 were measured in a total of 100 g at the same mass ratio as those of Example 1 in Table 1 (20:72=21.7:78.3). Silver particles and AG-2-1C were measured in a total of 100 g at the same mass ratio as those of Comparative Example 1 in Table 1 (20:72=21.7:78.3).

[0119] After each measurement, the mixture was stirred with a spatula and stirred for 30 seconds in a kneading and degassing machine. The revolution speed of the container of the kneading and degassing machine was 1400 rpm and the rotation speed was 700 rpm.

[0120] 0.5 g of the stirred silver particles were placed in a cylindrical container with an inner diameter of 5 mm and an open top, and a load of 2000 N was applied for 20 seconds to form a cylindrical sample with a diameter of 5 mm and a thickness of 3.5 to 3.7 mm.

[0121] For each of the obtained samples, thermomechanical analysis was performed under the following conditions.

[0122] Manufacturer: SII (Seiko Instruments Inc.)

[0123] Model: TMA / SS6200

[0124] Heating rate: 3℃ / min

[0125] Measuring temperature: 30~700℃

[0126] Measuring load: 700mN (probe area: φ3mm, equivalent to 0.1MPa)

[0127] Measurement atmosphere: Nitrogen gas was flowed into the thermomechanical analysis apparatus at a flow rate of 200 mL / min.

[0128] [Preparation of a joint body for evaluation]

[0129] The bonding materials of Example 1 and Comparative Example 1 prepared above were coated on a 30mm×30mm (1mm thick) copper substrate using a metal mask (opening 13.5mm×13.5mm, thickness 150μm). On the coating film of each bonding material formed on the copper substrate, a 13mm×13mm (0.3mm thick) Si element with a square bottom surface was placed. The element was heated from 25°C to 250°C at 3°C / min in a N2 atmosphere, and fired at this temperature for 60 minutes without pressure to form a silver bonding layer to obtain a bonded body.

[0130] <Pore Evaluation>

[0131] The bonding part of the Si element-silver bonding layer-copper substrate of each bonded body was photographed from the Si element side using an ultrasonic microscope (C-SAMD-9500, manufactured by Sonoscan) with a 50 MHz probe (converter). The obtained image was binarized using image processing software (trade name: PaintShop), and the area ratio of the pores between the Si element and the silver bonding layer in the area within 1.3 mm from each side of the Si element, which is within 20% of the distance from the center of the contact surface to the edge constituting its outline, was obtained. The black part was judged as having no pores, and the white part was judged as having pores.

[0132] The porosity in the region A when the bonding material of Example 6 was used was 8.1%, and the porosity in the region A when the bonding material of Comparative Example 8 was used was 45.2%.

[0133] [Table 2]

[0134]

Claims

1. A metal paste for bonding, comprising metal nanoparticles (A) having a primary particle size of 10 to 100 nm by number average, wherein the cumulative weight loss value (L 700 ) is set as 100, the cumulative value of the weight loss when the temperature is increased from 40℃ to 100℃ (L 100 ) is less than 75, and the cumulative value of weight loss when the temperature is increased from 40℃ to 150℃ (L 150 ) is above 90, and the cumulative value of weight loss when the temperature is increased from 40℃ to 200℃ (L 200 ) is 98 or above, When the total amount of the metal paste for bonding comprising metal particles containing metal nanoparticles (A), a solvent, a dispersant and other additives is set to 100 mass % and the calcination temperature is set to Tb (°C), the solvent having a boiling point or a decomposition temperature of greater than Tb-50 (°C) and less than Tb+50 (°C) accounts for greater than 5 mass % and less than 10 mass %.

2. The metal paste for bonding according to claim 1, wherein The cumulative value of weight loss when the temperature rises from 40℃ to 200℃ (L 200 ) is below 99.

9.

3. The metal paste for bonding according to claim 1 or 2, wherein When the total amount of the metal paste for bonding comprising metal particles containing metal nanoparticles (A), solvents, dispersants and other additives is set to 100 mass% and the calcination temperature is set to Tb (°C), it contains 1.5 mass% or less of components having a boiling point or decomposition temperature higher than the calcination temperature Tb+50 (°C).

4. The metal paste for bonding according to claim 1, comprising metal particles, wherein the metal particles include metal nanoparticles (A) having a primary particle size having a number average value of 10 to 100 nm, and the shrinkage of the metal particles contained in the paste measured in a thermomechanical analysis performed while being pressurized at 0.1 MPa in a nitrogen atmosphere and heated from 30°C to 250°C at a heating rate of 3°C / min is 1.5% or less.

5. The metal paste for bonding according to claim 4, wherein The shrinkage rate of the metal particles measured by thermomechanical analysis while the temperature was raised from 30° C. to 200° C. was 0.5% or less.

6. The metal paste for bonding according to claim 4 or 5, wherein The shrinkage rate of the metal particles measured by thermomechanical analysis while the temperature was raised from 30° C. to 175° C. was 0.3% or less.

7. The metal paste for bonding according to any one of claims 1 to 6, comprising a volume-converted average particle size (D 50 ) are metal particles (B) of 1.0 to 5.0 μm.

8. The metal paste for bonding according to claim 7, wherein The weight mixing ratio of the metal nanoparticles (A) to the metal particles (B) is (A) / (B) of 0.25 or less.

9. A method for joining two joined components, comprising the following steps: a step of coating the joining metal paste described in any one of claims 1 to 8 on the joined components; placing another joined component coated with the paste on another joined component on the coating; and a step of heating the component to a sintering temperature of 200 to 350°C after placement and maintaining the temperature at the sintering temperature for no more than 2 hours to form a metal joining layer. 10 . The bonding method according to claim 9 , comprising a step of drying the bonding metal paste at a temperature of 50 to 150° C. after applying the bonding metal paste.

11. The bonding method according to claim 9 or 10, wherein: The heating rate from room temperature to the sintering temperature is 1.5 to 10° C. per minute.

12. The bonding method according to any one of claims 9 to 11, wherein: The area where the metal paste for bonding is applied, i.e. the bonding area, is 9 mm 2 above.