Multi-level pore titanium silicon molecular sieve and preparation method thereof and method for catalytic oxidation of cyclohexene
By introducing a hierarchical pore structure into titanium-silicon molecular sieves and using silanization reagent treatment and hydrothermal crystallization technology, the problem of insufficient reaction activity of titanium-silicon molecular sieves in catalytic oxidation of cyclohexene was solved, and efficient cyclohexene conversion and cyclohexene oxidation were achieved. Improved selectivity of oxycyclohexane and cyclohexanediol.
Patent Information
- Application Number
- CN202111608088.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-12-22
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2041-12-22
AI Technical Summary
Existing titanium-silicon molecular sieves have insufficient catalytic activity in the catalytic oxidation of cyclohexene. In particular, the epoxidation reaction efficiency of macromolecular olefins is low, and the introduction of too many mesoporous channels will lead to the loss of active centers and affect the catalytic performance.
The titanium silica sol is treated with a specific silanization reagent to prepare hierarchical porous titanium silica molecular sieves. Hydrothermal crystallization and roasting methods are used to form a stable organic-inorganic support layer structure and improve the microporous and mesoporous structure of the titanium silica molecular sieves. Thereby improving the efficiency of catalytic oxidation of cyclohexene.
Significantly increased the cyclohexene conversion rate to more than 90%, the epoxycyclohexane selectivity to more than 41%, and the cyclohexanediol selectivity to more than 44%, improving the catalytic activity and selectivity.
Smart Images

Figure CN116332195B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of catalytic oxidation of cyclohexene, and in particular to a multi-level porous titanium silicon molecular sieve and a preparation method thereof and a method for catalytic oxidation of cyclohexene. Background Art
[0002] 1,2-cyclohexanediol, a white crystalline substance, is slightly soluble in water, soluble in ethanol, ethyl acetate, etc. It is an important organic chemical raw material and solvent. 1,2-cyclohexanediol is an important organic synthetic raw material and can be used to prepare a variety of intermediates, mainly used in pesticides, medicines, chemical additives, etc. For example, 1,2-cyclohexanediol can be used as a raw material for high-grade diluents of epoxy resins. In addition, it can be used as a raw material to produce unsaturated polyester resins and powder coatings. It can also be used to produce dyes, pesticides, pharmaceutical intermediates, plasticizers, flame retardants, etc.
[0003] Epoxycyclohexane, also known as cyclohexene oxide, is a colorless or light yellow liquid, slightly soluble in water, and easily soluble in alcohol, ketone and a variety of organic solvents. Epoxycyclohexane can be used as an active diluent for epoxy resins, an intermediate for synthetic pesticides, and can also be used as a raw material to prepare surfactants, rubber additives, etc. The epoxy group of epoxycyclohexane is very active. It can react with alcohols, carboxylic acids, phenols, etc. to obtain a series of high value-added products, which are used in the fields of medicine and pesticides. The production methods of epoxycyclohexane include hypochlorous acid oxidation method, cyclohexene oxidation method, cyclohexanone method, etc. Considering the needs of environmental protection and green chemistry, cyclohexene oxidation method has gradually been developed. According to the different oxidants used in the cyclohexene oxidation process, cyclohexene oxidation can be divided into organic peroxyacid method, inorganic peroxyacid method and catalytic oxidation method, among which catalytic oxidation method is more efficient, especially hydrogen peroxide oxidation method, which is the most concerned. Hydrogen peroxide oxidation only generates water after the hydrogen peroxide reaction, which is pollution-free to the environment and is a green oxidant. Titanium silicate molecular sieve and hydrogen peroxide can form an efficient catalytic oxidation system (Ti-OOH), which has a good catalytic effect on the synthesis of various epoxides.
[0004] Titanium silicate molecular sieve has uniform pores, large specific surface area and special active centers, and is widely used in the field of catalysis. The TS-1 molecular sieve currently in industrial production has an MFI topological structure, and its ten-membered ring pore diameter is about 0.56nm, and small molecule olefins can more easily enter the pores and contact the catalytic active centers. In order to promote the catalytic epoxidation reaction of macromolecular olefins by titanium silicate molecular sieve, researchers have explored the preparation of multi-level pore titanium silicate molecular sieves. CN108726528A discloses a multi-level pore titanium silicate molecular sieve, a preparation method thereof and a method for olefin epoxidation. A certain proportion of mesoporous channels can be introduced into the titanium silicate molecular sieve by treatment with a silanizing agent, but the introduction of too many mesoporous channels will lead to the loss of some active centers, which may lead to a decrease in catalytic activity. Summary of the invention
[0005] The purpose of the present invention is to improve the catalytic oxidation performance of titanium silicate in the catalytic oxidation of cyclohexene, and to provide a multi-level pore titanium silicate and a preparation method thereof and a method for catalytic oxidation of cyclohexene.
[0006] In order to achieve the above object, the first aspect of the present invention provides a method for preparing a multi-level porous titanium silicon molecular sieve, the method comprising:
[0007] (1) mixing a silicon source, an alkaline template, a titanium source and water to obtain a titanium silicalose;
[0008] (2) adding the compound represented by formula (I) to the titanium silicalose sol, and subjecting the obtained mixture to hydrothermal crystallization and calcination;
[0009]
[0010] Wherein, i is an integer of 1-10; R1, R2 and R3 are each independently selected from a C1-C6 alkyl group.
[0011] The second aspect of the present invention provides a multi-level pore titanium silicon molecular sieve prepared according to the method described in the first aspect.
[0012] The third aspect of the present invention provides a method for catalytic oxidation of cyclohexene, the method comprising: contacting cyclohexene, a catalyst, methanol and hydrogen peroxide for reaction, wherein the catalyst comprises the multi-level porous titanium silicon molecular sieve described in the second aspect.
[0013] Through the above technical scheme, the present invention treats the titanium silicalite precursor with a specific silanization reagent, and the prepared titanium silicalite has high catalytic activity when used for catalytic oxidation of cyclohexene. The cyclohexene conversion rate is increased to more than 90%, the selectivity of cyclohexene oxide is increased to more than 41%, and the selectivity of cyclohexanediol is increased to more than 44%. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] Figure 1 is the XRD spectrum of the multi-level pore titanium silicon molecular sieve obtained in Example 1 of the present invention;
[0015] Figure 2 is the UV-Vis spectrum of the hierarchical pore titanium silicalite molecular sieve obtained in Example 1 of the present invention;
[0016] Figure 3 is a TEM image of the multi-level pore titanium silicon molecular sieve obtained in Example 1 of the present invention;
[0017] Figure 4 This is the XRD spectrum of the titanium silicon molecular sieve obtained in Comparative Example 1. DETAILED DESCRIPTION
[0018] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0019] As mentioned above, the first aspect of the present invention provides a method for preparing a multi-level porous titanium silicon molecular sieve, the method comprising:
[0020] (1) mixing a silicon source, an alkaline template, a titanium source and water to obtain a titanium silicalose;
[0021] (2) adding the compound represented by formula (I) to the titanium silicalose sol, and subjecting the obtained mixture to hydrothermal crystallization and calcination;
[0022]
[0023] Wherein, i is an integer of 1-10; R1, R2 and R3 are each independently selected from a C1-C6 alkyl group.
[0024] In the present invention, the C1-C6 alkyl group refers to an alkyl group having 1 to 6 carbon atoms in total, for example, it can be one of methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, tert-butyl, n-pentyl and n-hexyl.
[0025] In some preferred embodiments of the present invention, i is an integer of 1-5, for example, 1, 2, 3, 4 or 5.
[0026] In some preferred embodiments of the present invention, R1, R2 and R3 are each independently selected from a C1-C3 alkyl group, and the C1-C3 alkyl group may be a methyl group, an ethyl group, a n-propyl group or an isopropyl group. Preferably, R1, R2 and R3 are each independently selected from a methyl group, an ethyl group or an n-propyl group. In the present invention, R1, R2 and R3 may be the same or different. Preferably, R1, R2 and R3 are the same.
[0027] The present invention adopts a compound represented by formula (I) as a silanization agent, wherein the chlorine-containing group in the silanization agent can be substituted with a hydroxide ion, and further hydrolyzed to generate a hydroxyl group; through the condensation reaction of the hydroxyl groups in a plurality of molecules, a stable organic-inorganic supporting layer structure can be generated inside the titanium silicalite during the hydrothermal crystallization process, so that the titanium silicalite has not only a microporous structure but also a mesoporous structure, thereby facilitating the intracrystalline and intercrystalline mass transfer and diffusion of reactant molecules and product molecules in the catalytic oxidation of cyclohexene, and effectively improving the cyclohexene conversion rate, the selectivity of cyclohexene oxide and the selectivity of cyclohexanediol.
[0028] According to the present invention, if the amount of the silanization agent (the compound shown in formula (I)) is too high, the crystallization performance of the titanium silicalite will deteriorate; if the amount of the silanization agent (the compound shown in formula (I)) is too low, the specific surface area of the titanium silicalite molecular sieve will be reduced, and the mesoporous structure of the titanium silicalite molecular sieve may also change, affecting mass transfer and further affecting its catalytic activity in the cyclohexene oxidation reaction; under preferred conditions, in step (1), the silicon source is calculated as SiO2, and the molar ratio of the silicon source to the compound shown in formula (I) is 1:(0.01-0.3), preferably 1:(0.01-0.2); more preferably 1:(0.05-0.2).
[0029] In some preferred embodiments of the present invention, the silicon source is calculated as SiO2, the alkaline template is calculated as N when it contains nitrogen, and the alkaline template is calculated as OH when it does not contain nitrogen. - The molar ratio of the silicon source, the alkaline template and water is 1:(0.05-0.4):(5-40); preferably 1:(0.1-0.3):(5-25).
[0030] According to the present invention, under preferred conditions, the silicon source is selected from at least one of tetramethyl silicate, tetraethyl silicate, tetrapropyl silicate, tetrabutyl silicate, white carbon black and silica sol;
[0031] According to the present invention, under preferred conditions, the alkaline template agent is selected from at least one of quaternary ammonium bases, aliphatic amines and aliphatic alcohol amines, preferably at least one of tetramethylammonium hydroxide, tetraethylammonium hydroxide, tetrapropylammonium hydroxide and tetrabutylammonium hydroxide;
[0032] In some preferred embodiments of the present invention, the silicon source is calculated as SiO2, the titanium source is calculated as TiO2, and the molar ratio of the silicon source to the titanium source is 1:(0.001-0.04), preferably 1:(0.005-0.025).
[0033] According to the present invention, under preferred conditions, the titanium source is selected from an organic titanium source and / or an inorganic titanium source; further preferably, the titanium source is selected from at least one of titanium tetrachloride, titanium sulfate, titanium nitrate, tetraethyl titanate, tetrapropyl titanate and tetrabutyl titanate.
[0034] In a preferred embodiment of the present invention, step (1) further comprises: mixing the silicon source, the alkaline template and water, and performing a first stirring at room temperature for 0.1-2 hours, then adding the titanium source during the stirring process, and performing a second stirring for 0.5-6 hours to obtain titanium silicalose. Under preferred conditions, the second stirring time is 0.5-3 hours, more preferably 1-2.5 hours.
[0035] According to the present invention, under preferred conditions, step (1) further comprises: driving out alcohol after the mixing; driving out alcohol can remove alcohol generated by hydrolysis of silicon source and titanium source, and in the present invention, preferably azeotropic distillation is used to remove alcohol generated in the system, and water lost by azeotropic distillation is supplemented during the driving out alcohol process to ensure that the ratio of each substance in the titanium silica sol meets the above requirements; preferably, the conditions for driving out alcohol include: temperature of 30-100°C and time of 2-10h; more preferably: temperature of 40-90°C and time of 4-10h.
[0036] According to the present invention, in order to make the silanization agent uniformly dispersed in the titanium silica sol, under preferred conditions, step (1) also includes: adding the compound represented by formula (I) to the titanium silica sol and performing a third stirring for 0.1-24 hours, preferably the third stirring time is 0.5-10 hours, and more preferably 1-3 hours.
[0037] The nucleation and growth rates of the titanium silicon molecular sieve can be controlled by rapidly heating up to obtain a titanium silicon molecular sieve with a smaller size. Under preferred conditions, in step (2), the conditions for the hydrothermal crystallization include: heating the mixture to 50-200°C within 0.1-1h, and then performing hydrothermal crystallization at 50-200°C for 10-100h; preferably, performing hydrothermal crystallization at a temperature of 100-200°C for 20-80h; further preferably, the heating time is 0.3-0.6h; more preferably, the conditions for the hydrothermal crystallization include: a temperature of 150-180°C and a time of 20-48h; under the above preferred conditions, the crystallinity, specific surface area and pore volume of the molecular sieve can be balanced to obtain a molecular sieve with specific crystallinity, specific surface area and pore volume.
[0038] The present invention has no particular limitation on the pressure of hydrothermal crystallization, which may be the autogenous pressure of the crystallization system.
[0039] According to the present invention, under preferred conditions, the method further comprises: washing, filtering and drying the product obtained by hydrothermal crystallization; wherein the washing, filtering and drying processes can be known to those skilled in the art. Exemplarily, the washing temperature can be 20-50°C, the washing solvent can be water, and the amount of the washing solvent is 1-20 times the mass of the crystallized product; the drying conditions can be: the temperature is 40-150°C and the time is 0.5-24h.
[0040] In some preferred embodiments of the present invention, the calcination conditions include: a temperature of 400-800° C. and a time of 1-15 h; preferably a temperature of 500-600° C. and a time of 4-10 h.
[0041] The second aspect of the present invention provides a multi-level pore titanium silicon molecular sieve prepared according to the method described in the first aspect.
[0042] According to the present invention, under preferred conditions, the crystallinity of the multi-level pore titanium silicon molecular sieve is 65-75%; the particle size is 100-250nm; the mesopore volume is 0.35-0.45g / cm 3 ; Micropore volume is 0.17-0.23g / cm 3 .
[0043] Further preferably, there are mesopores of various pore sizes in the multi-level pore titanium silicalite, and the pore size of the mesopores is 3-6nm or 40-50nm; and the pore volume of the mesopores with a pore size of 3-6nm accounts for 20-35% of the total mesopore volume; the pore volume of the mesopores with a pore size of 40-50nm accounts for 35-45% of the total mesopore volume.
[0044] According to the present invention, under preferred conditions, the diameter of the micropores in the multi-level pore titanium silicalite molecular sieve is 0.5-0.6 nm.
[0045] Further preferably, the molar ratio of silicon to titanium in the hierarchical pore titanium silicon molecular sieve is 1:0.001-0.04; preferably 1:0.005-0.025.
[0046] The third aspect of the present invention provides a method for catalytic oxidation of cyclohexene, the method comprising: contacting cyclohexene, a catalyst, methanol and hydrogen peroxide for reaction, wherein the catalyst comprises the multi-level porous titanium silicon molecular sieve described in the second aspect.
[0047] According to the present invention, under preferred conditions, the conditions for catalytic oxidation of cyclohexene include: temperature of 50-120° C., a molar ratio of cyclohexene to hydrogen peroxide of (2-5):1, and a molar ratio of catalyst, cyclohexene and methanol of 1:(10-30):(80-120).
[0048] In some embodiments of the present invention, the form of the catalyst can be selected according to actual needs. The catalyst can be a molecular sieve supported on a carrier or a molecular sieve powder. In the present invention, it is preferred to directly use the molecular sieve powder as the catalyst.
[0049] According to a particularly preferred embodiment of the present invention, the method for preparing titanium silicon molecular sieve comprises:
[0050] (1) mixing a silicon source, an alkaline template and water at a molar ratio of 1:(0.1-0.3):(5-25), performing a first stirring at room temperature for 0.1-2 hours, then adding a titanium source during the stirring process, and performing a second stirring for 1-2.5 hours to obtain a mixed system; wherein the molar ratio of the silicon source to the titanium source is 1:(0.005-0.025);
[0051] Then, the mixed system is subjected to alcohol removal to obtain titanium silicalose; the temperature of the alcohol removal is 40-90° C. and the time is 4-10 hours;
[0052] (2) adding the compound represented by formula (I) to the titanium silicalose sol and performing a third stirring for 1-3 hours, and performing hydrothermal crystallization and calcination on the obtained mixture; wherein the molar ratio of the silicon source to the compound represented by formula (I) is 1:(0.03-0.2), and the crystallization conditions are: heating the mixture to 150-180° C. within 0.3-0.6 hours, and then performing hydrothermal crystallization at 150-180° C. for 20-48 hours;
[0053]
[0054] Wherein, i is an integer of 1-5; R1, R2 and R3 are the same; R1, R2 and R3 are selected from methyl, ethyl or propyl.
[0055] The present invention will be described in detail below by way of examples. In the following examples, room temperature refers to 25±5°C.
[0056] In the following embodiments and comparative examples, the X-ray diffraction (XRD) crystal phase diagram of the samples was measured on a Siemens D5005 X-ray diffractometer, the ray source was Cu Kα, the tube voltage was 40 kV, the tube current was 40 mA, the scanning speed was 0.5° / min, and the scanning range was 2θ=5°-35°; according to the XRD spectrum, the crystallinity was obtained by fitting the software eva independently developed by BRUKER;
[0057] The UV-Vis spectra (UV-Vis) of the samples were obtained by Agilent Cary 300 UV spectrophotometer with a wavelength interval of 3 nm and a scanning range of 190-800 nm;
[0058] The pore volume was determined according to the method described in RIPP 151-90 in "Analytical Methods in Petrochemical Industry" compiled by Yang Cuiding et al. (Science Press, first edition, published in September 1990);
[0059] The pore size distribution was calculated according to the BJH formula;
[0060] The size of the molecular sieves was characterized by JEOL JEM-2100 transmission electron microscope (TEM).
[0061] In the following examples, the silanization agents used are shown in Table 1; Compound 1, Compound 2 and Compound 3 were all purchased commercially.
[0062] Table 1
[0063]
[0064]
[0065] Example 1
[0066] (1) Tetramethyl silicate, tetrapropylammonium hydroxide and water are first stirred at room temperature for 0.5 h, and tetraethyl titanate is added during the stirring process, and a second stirring is performed for 2.5 h to obtain a mixed system; wherein tetramethyl silicate is calculated as SiO2, tetrapropylammonium hydroxide is calculated as N, tetraethyl titanate is calculated as TiO2, and the molar ratio of tetramethyl silicate, tetrapropylammonium hydroxide, water and tetraethyl titanate is 1:0.15:15:0.01;
[0067] Then, the mixed system was subjected to alcoholization at 60°C for 7 hours to obtain titanium silicalose;
[0068] (2) adding compound (1) to titanium silicalose, and stirring for a third time at room temperature for 3 hours to obtain a mixture, wherein the molar ratio of compound (1) to tetramethyl silicate is 0.15:1;
[0069] (3) heating the mixture to 170° C. for 0.3 h, and performing hydrothermal crystallization at 170° C. for 48 h to obtain a crystallized product;
[0070] The crystallized product was sequentially washed with water, filtered, and dried at 120 °C for 2 h;
[0071] The dried product was calcined at 550°C for 6 h to obtain a hierarchical pore titanium silicon molecular sieve, the physical properties of which are shown in Table 3;
[0072] The XRD spectrum of the multi-level pore titanium silicon molecular sieve obtained in this example is as follows: Figure 1 As shown, from Figure 1 It can be seen that the multi-level pore titanium silicon molecular sieve of this embodiment has an MFI structure;
[0073] The UV-Vis spectrum of the multi-level pore titanium silicate molecular sieve obtained in this example is as follows: Figure 2 As shown, from Figure 2 It can be seen that the hierarchical pore titanium silicon molecular sieve of the present embodiment has a framework Ti active center;
[0074] The TEM image of the multi-level pore titanium silicon molecular sieve obtained in this example is as follows: Figure 3 As shown, from Figure 2 It can be seen that the particle size of the multi-level pore titanium silicon molecular sieve of this embodiment is about 100-200nm.
[0075] Example 2-20
[0076] Titanium silicate molecular sieve was prepared according to the method of Example 1. The proportions and synthesis conditions are shown in Table 2. The physical properties of the prepared multi-level pore molecular sieve are shown in Table 3.
[0077] Comparative Example 1
[0078] Titanium silicate molecular sieve was prepared according to the method for preparing titanium silicate micro-mesoporous molecular sieve composite material disclosed in "Zeolites, 1992, Vol. 12, pp. 943-950". The specific method is as follows:
[0079] Mix 22.5g of tetraethyl silicate, 7.0g of tetrapropylammonium hydroxide and 59.8g of deionized water evenly and hydrolyze at 60°C for 1.0h. Then, slowly drip a solution consisting of 1.1g of tetrabutyl titanate and 5.0g of isopropanol into the above solution under vigorous stirring, and stir the mixture at 75°C for 3h to obtain a clear and transparent colloid. Then move the colloid into a stainless steel closed reactor and crystallize it at a constant temperature of 170°C for 72h to obtain a conventional TS-1 molecular sieve. Its XRD analysis spectrum is shown as follows: Figure 4 shown.
[0080] Comparative Examples 2-6
[0081] Titanium silicate molecular sieve was prepared according to the method of Example 1. Its components and synthesis conditions are shown in Table 2. The physical properties of the prepared molecular sieve are shown in Table 3.
[0082] Comparative Example 7
[0083] Titanium silicate molecular sieve was prepared according to the method of Example 1, except that the silanization agent was tert-butyldimethylsilyl chloride (Compound 4); its components and synthesis conditions are shown in Table 2, and the physical properties of the prepared molecular sieve are shown in Table 3.
[0084] Comparative Example 8
[0085] Titanium silicate molecular sieve was prepared according to the method of Example 1, except that the silanization agent was trimethylchlorosilane (Compound 5). Its components and synthesis conditions are shown in Table 2. The physical properties of the prepared molecular sieve are shown in Table 3.
[0086]
[0087] Table 3
[0088]
[0089] Note: **3-6nm refers to the proportion of the pore volume of mesopores with a pore size of 3-6nm to the total mesopore volume;
[0090] **8-12nm refers to the proportion of the pore volume of mesopores with a pore size of 8-12nm to the total mesopore volume;
[0091] **40-60nm refers to the proportion of the pore volume of mesopores with a pore size of 40-50nm to the total mesopore volume.
[0092] Test Case
[0093] This test example illustrates the reaction effect of the sample of the embodiment provided by the present invention and the sample prepared in the comparative example for the oxidation of cyclohexene to prepare epoxycyclohexane and cyclohexanediol. The reagents used in this test example are all commercially available chemically pure reagents. The concentration of each substance after the reaction is quantitatively analyzed using gas chromatography. The 6890 gas chromatograph produced by Agilent was used; the analytical chromatographic column used was an FFAP column. The component concentration was quantified using the external standard method. First, the peak area of each component was measured, the component concentration was obtained through the standard working curve, and each index was calculated.
[0094] The cyclohexene conversion, cyclohexene oxide and cyclohexanediol selectivity in the test example were calculated according to the following formulas:
[0095] Cyclohexene conversion rate % = (1-moles of cyclohexene remaining after reaction / moles of cyclohexene added before reaction) × 100%
[0096] Cyclohexene oxide selectivity % = moles of cyclohexene oxide after reaction / (moles of cyclohexene added before reaction - moles of cyclohexene remaining after reaction) × 100%
[0097] Cyclohexanediol selectivity % = moles of cyclohexanediol after reaction / (moles of cyclohexene added before reaction - moles of cyclohexene remaining after reaction) × 100%
[0098] The molecular sieves prepared in the above Examples 1-20 and Comparative Examples 1-8 were added to a three-necked flask reaction vessel containing cyclohexene and methanol, wherein the molar ratio of the molecular sieve, cyclohexene, and methanol was 1:20:100. After the temperature stabilized to the set value, hydrogen peroxide (concentration 30% by weight) was added, and the molar ratio of cyclohexene to hydrogen peroxide (in terms of H2O2) was 1:1. Then, the temperature was 80°C and the pressure was 0.1 MPa (normal pressure). After 6 hours of reaction, the experiment was stopped, the catalyst was filtered out, and samples were taken for chromatographic analysis. The reaction results are shown in Table 4.
[0099] As can be seen from Table 4, the cyclohexene epoxidation activity of the sample obtained in the present invention is significantly higher than that of the comparative sample conventional TS-1 molecular sieve.
[0100] Table 4
[0101]
[0102]
[0103] As can be seen from Table 4, the hierarchical pore titanium silicon molecular sieve prepared in the embodiment of the present invention has an epoxidation activity of cyclohexene of more than 90%; the selectivity of cyclohexene oxide is more than 41% and the selectivity of cyclohexanediol is more than 42%, which are significantly higher than the comparative example.
[0104] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A method for preparing a multi-level porous titanium silicon molecular sieve, It is characterized in that The method comprises: (1) mixing a silicon source, an alkaline template, a titanium source and water uniformly to obtain a titanium silicalite; (2) adding the compound represented by formula (I) to the titanium silicalose sol, and subjecting the obtained mixture to hydrothermal crystallization and calcination; Formula (I) Wherein, i is an integer from 1 to 10; R 1 , R 2 and R 3 Each independently selected from C 1 -C 6 The alkyl group; The silicon source is SiO 2 The molar ratio of the silicon source to the compound represented by formula (I) is 1:(0.01-0.3); The silicon source is SiO 2 When the alkaline template contains nitrogen, it is calculated as N; when the alkaline template does not contain nitrogen, it is calculated as OH - The titanium source is TiO 2 count, The molar ratio of the silicon source, the alkaline template and water is 1:(0.05-0.4):(5-40); and / or, the molar ratio of the silicon source to the titanium source is 1:(0.001-0.04); In step (2), the hydrothermal crystallization conditions include: heating the mixture to 50-200°C within 0.1-1h, and then crystallizing at 50-200°C for 10-100h; The multi-level pore titanium silicon molecular sieve prepared by the method has a crystallinity of 65-75%, a particle size of 100-250 nm, and a mesopore volume of 0.35-0.45 g / cm 3 ; Micropore volume is 0.17-0.23 g / cm 3 ; The multi-level pore titanium silicalite prepared by the method has mesopores of various pore sizes, wherein the pore size of the mesopores is 3-6nm or 40-50nm; the pore volume of the mesopores with a pore size of 3-6nm accounts for 20-35% of the total mesopore volume; and the pore volume of the mesopores with a pore size of 40-50nm accounts for 35-45% of the total mesopore volume.
2. The method according to claim 1, in, i is an integer from 1 to 5.
3. The method according to claim 1, in, R 1 , R 2 and R 3 Each is independently selected from methyl, ethyl or propyl.
4. The method according to claim 1, in, The silicon source is SiO 2 The molar ratio of the silicon source to the compound represented by formula (I) is 1:(0.01-0.2).
5. The method according to any one of claims 1 to 4, in, The silicon source is SiO 2 When the alkaline template contains nitrogen, it is calculated as N; when the alkaline template does not contain nitrogen, it is calculated as OH - The titanium source is TiO 2 count, The molar ratio of the silicon source, the alkaline template and water is 1:(0.1-0.3):(5-25); And / or, the molar ratio of the silicon source to the titanium source is 1:(0.005-0.025).
6. The method according to any one of claims 1 to 4, in, The silicon source is selected from at least one of tetramethyl silicate, tetraethyl silicate, tetrapropyl silicate, tetrabutyl silicate, white carbon black and silica sol.
7. The method according to any one of claims 1 to 4, in, The alkaline template agent is selected from at least one of quaternary ammonium base, aliphatic amine and aliphatic alcohol amine.
8. The method according to claim 7, in, The alkaline template agent is at least one of tetramethylammonium hydroxide, tetraethylammonium hydroxide, tetrapropylammonium hydroxide and tetrabutylammonium hydroxide.
9. The method according to any one of claims 1 to 4, in, The titanium source is selected from an organic titanium source and / or an inorganic titanium source.
10. The method according to claim 9, in, The titanium source is selected from at least one of titanium tetrachloride, titanium sulfate, titanium nitrate, tetraethyl titanate, tetrapropyl titanate and tetrabutyl titanate.
11. The method according to any one of claims 1 to 4, in, Step (1) also includes removing alcohol after the mixing.
12. The method according to claim 11, in, The conditions for driving out the alcohol include: temperature of 30-100° C. and time of 2-10 h.
13. The method according to claim 12, in, The conditions for driving out the alcohol include: temperature of 40-90° C. and time of 4-10 h.
14. The method according to any one of claims 1 to 4, in, In step (2), the hydrothermal crystallization conditions include: performing crystallization at a temperature of 100-200° C. for 20-80 hours.
15. The method according to any one of claims 1 to 4, in, The calcination conditions include: temperature of 400-800° C. and time of 1-15 hours.
16. A hierarchical pore titanium silicon molecular sieve prepared according to the method according to any one of claims 1 to 15.
17. The multi-level pore titanium silicon molecular sieve according to claim 16, in, The molar ratio of silicon to titanium in the multi-level porous titanium silicon molecular sieve is 1:0.001-0.
04.
18. The multi-level pore titanium silicon molecular sieve according to claim 17, in, The molar ratio of silicon to titanium in the multi-level porous titanium silicon molecular sieve is 1:0.005-0.
025.
19. A method for catalytic oxidation of cyclohexene, the method comprising: include: Cyclohexene, a catalyst, methanol and hydrogen peroxide are contacted to react, wherein the catalyst comprises the multi-level porous titanium silicon molecular sieve according to any one of claims 16 to 18.
20. The method according to claim 19, in, The conditions for catalytic oxidation of cyclohexene include: a temperature of 50-120° C., a molar ratio of cyclohexene to hydrogen peroxide of (2-5):1, and a molar ratio of catalyst, cyclohexene and methanol of 1:(10-30):(80-120).
Citation Information
Patent Citations
Hierarchical porous titanium-silicon molecular sieve as well as preparation method thereof and olefin epoxidation method
CN108726528A
Interior surface coating structure mesoporous titanium silicate molecular sieve material and preparation method and use thereof
CN101417809A
Preparation method and application of hierarchical zeolite molecular sieve
CN103073020A
Self-forming technology of titanium silicalite molecular sieve TS-1
CN104986782A
Preparation method of hierarchical porous titanium silicon molecular sieve
CN106145149A