Multi-level pore titanium silicon molecular sieve and preparation method thereof and method for epoxidation of monoolefins

By using specific silanization reagents in titanium silica sol for hydrothermal crystallization, hierarchical porous titanium silica molecular sieves were prepared, which solved the problem of insufficient catalytic activity of titanium silica molecular sieves, improved the conversion rate and selectivity of monoolefins, and Reduced costs.

CN116332199BActive Publication Date: 2024-10-25CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202111579904.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-22
Publication Date
2024-10-25
Estimated Expiration
2041-12-22

AI Technical Summary

Technical Problem

Existing titanium-silicon molecular sieves have insufficient catalytic activity in monoolefin epoxidation reactions, and traditional preparation methods lead to imperfect structures or high costs.

Method used

By adding specific silanization reagents to titanium silica sol for hydrothermal crystallization and roasting, a hierarchical porous titanium silicon molecular sieve with 5-10nm mesopores and 0.1-2nm micropores is prepared to improve the catalytic activity.

Benefits of technology

The conversion rate of monoolefins is over 91%, which improves the selectivity of the product and reduces the preparation cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116332199B_ABST
    Figure CN116332199B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of olefin epoxidation, and in particular to a multi-level porous titanium silicon molecular sieve and a preparation method thereof and a method for epoxidation of monoolefins. The multi-level porous titanium silicon molecular sieve has a mesopore diameter of 5-10 nm and a specific surface area of ​​500-650 m 2 / g, with a total pore volume of 0.45-0.8cm 3 / g, with an external surface area of ​​120‑300m 2 / g, micropore volume is 0.12-0.2cm 3 / g, the particle size of the molecular sieve particles is 100-250nm, and the molecular sieve crystallinity is ≥50%. The present invention treats the titanium silicalite precursor with a specific silanization agent, and the prepared titanium silicalite has a mesoporous channel with a pore size of 5-10nm and a large specific surface area and pore volume. When the titanium silicalite is used in the epoxidation reaction of monoolefins, it has high catalytic activity, and the conversion rate of monoolefins can be increased to more than 91%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of olefin epoxidation, and in particular to a multi-level porous titanium silicon molecular sieve and a preparation method thereof and a method for epoxidation of monoolefins. Background Art

[0002] Titanium silicate molecular sieve is composed of silicon-oxygen tetrahedron and titanium-oxygen tetrahedron, and is a kind of porous inorganic material with catalytic oxidation performance. The catalytic oxidation performance of titanium silicate molecular sieve depends on the titanium atoms in the form of tetracoordination in the framework structure. These isolated titanium atoms can catalyze the epoxidation reaction of various olefins under mild reaction conditions, and have the advantages of environmental friendliness, cleanliness, high efficiency, and high product selectivity. Among them, the typical titanium silicate molecular sieve catalyst is TS-1 molecular sieve. TS-1 molecular sieve has an MFI topological structure with a five-membered ring as the basic unit, and its unique pore structure can improve product selectivity. In view of the successful industrial preparation of TS-1, its application field has gradually broadened, and the types of catalytic reactions have gradually enriched. The narrow ten-membered ring pores of traditional TS-1 molecular sieves can no longer meet the needs of organic macromolecular reactions. Therefore, it is urgent to develop multi-level pore TS-1 molecular sieves. Common methods for synthesizing multi-level pore TS-1 molecular sieves include framework atom removal method, hard template method and soft template method. The skeleton atom removal method refers to a method of producing mesopores by dissolving the molecular sieve skeleton with an alkaline solution, but this method inevitably leads to the loss of some active centers, and the loss of the skeleton structure leads to a decrease in the structural stability of the molecular sieve. The hard template method refers to a method of adding a hard template agent to the titanium silical sol to produce mesopores through the occupying effect. However, the hard template agent is easily repelled by the titanium silical sol, so that it cannot be completely embedded to produce uniform mesopores. The soft template method is a method of expanding the pores using a soft template agent. The soft template agent has good hydrophilicity and can interact with the titanium silical sol to form mesoporous channels with good penetration, but it is expensive and has a high cost.

[0003] CN108726528A discloses a multi-level porous titanium silicate molecular sieve and a preparation method thereof and a method for olefin epoxidation. A certain proportion of mesoporous channels can be introduced into the titanium silicate molecular sieve by treatment with a silanization agent, but the introduction of a larger mesoporous structure will lead to an imperfect molecular sieve structure, and a larger particle size is not conducive to the diffusion of reaction molecules. Summary of the invention

[0004] The purpose of the present invention is to improve the catalytic oxidation activity of titanium silicate in the epoxidation reaction of monoolefins, and to provide a multi-level pore titanium silicate and a preparation method thereof and a method for epoxidation of monoolefins.

[0005] In order to achieve the above object, the present invention provides a multi-level pore titanium silicon molecular sieve in the first aspect, wherein the mesopore diameter of the multi-level pore titanium silicon molecular sieve is 5-10nm, the specific surface area is 500-650m 2 / g, with a total pore volume of 0.45-0.8cm3 / g, with an external surface area of ​​120-300m 2 / g, micropore diameter is 0.1-2nm, micropore volume is 0.12-0.2cm 3 / g, the particle size of the molecular sieve particles is 100-250nm, and the crystallinity of the molecular sieve is ≥50%.

[0006] A second aspect of the present invention provides a method for preparing a multi-level porous titanium silicon molecular sieve, the method comprising:

[0007] (1) mixing a silicon source, an alkaline template, a titanium source, water and isopropanol to obtain a titanium silicalose sol;

[0008] (2) adding the compound represented by formula (I) to the titanium silicalose sol, and subjecting the obtained mixture to hydrothermal crystallization and calcination;

[0009]

[0010] Wherein, i is an integer of 0-10; R1, R2 and R3 are each independently selected from a C1-C6 alkyl group.

[0011] The third aspect of the present invention provides a multi-level pore titanium silicon molecular sieve prepared according to the method described in the second aspect.

[0012] The fourth aspect of the present invention provides a method for epoxidation of a monoolefin, the method comprising: contacting a monoolefin and a peroxide for reaction in the presence of a catalyst, wherein the catalyst comprises the multi-level porous titanium silicon molecular sieve described in the first aspect or the third aspect.

[0013] Through the above technical scheme, the present invention treats the titanium silicalite precursor with a specific silanization reagent, and the prepared titanium silicalite has mesoporous channels with a pore size of 5-10nm, microporous channels with a pore size of 0.1-2nm, and a large specific surface area and pore volume. When the titanium silicalite is used in the epoxidation reaction of monoolefins, it has high catalytic activity, and the conversion rate of monoolefins can be increased to more than 91%. BRIEF DESCRIPTION OF THE DRAWINGS

[0014] Figure 1 is a pore size distribution diagram of the titanium silicon molecular sieve obtained in Example 1 of the present invention;

[0015] Figure 2 is a N2 adsorption-desorption curve diagram of the titanium silicon molecular sieve obtained in Example 1 of the present invention;

[0016] Figure 3 is a TEM image of the titanium silicon molecular sieve obtained in Example 1 of the present invention;

[0017] Figure 4 is the XRD diagram of the titanium silicon molecular sieve obtained in Example 1 of the present invention;

[0018] Figure 5 This is the pore size distribution diagram of the titanium silicon molecular sieve obtained in Comparative Example 1. DETAILED DESCRIPTION

[0019] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0020] As mentioned above, the first aspect of the present invention provides a multi-level porous titanium silicon molecular sieve, wherein the mesopore diameter of the multi-level porous titanium silicon molecular sieve is 5-10nm, the specific surface area is 500-650m 2 / g, with a total pore volume of 0.45-0.8cm 3 / g, with an external surface area of ​​120-300m 2 / g, micropore diameter is 0.1-2nm; micropore volume is 0.12-0.2cm 3 / g, the particle size of the molecular sieve particles is 100-250nm, and the crystallinity of the molecular sieve is ≥50%.

[0021] In the present invention, the external surface area of ​​the titanium silicalite molecular sieve refers to the surface area of ​​the outer surface of the titanium silicalite molecular sieve, which can be obtained by testing using the BET method; the specific surface area of ​​the titanium silicalite molecular sieve refers to the BET specific surface area.

[0022] According to the present invention, under preferred conditions, the molar ratio of titanium to silicon in the multi-level porous titanium silicon molecular sieve is 0.001-0.04:1; preferably 0.005-0.025:1.

[0023] In some preferred embodiments of the present invention, the infrared spectrum of the multi-level porous titanium silicon molecular sieve has a wave number of 960 cm -1 The peak area and wave number of 800cm -1 The ratio of the peak area (I 960 / I 800 ) is 0.7-2.

[0024] A second aspect of the present invention provides a method for preparing a multi-level porous titanium silicon molecular sieve, the method comprising:

[0025] (1) mixing a silicon source, an alkaline template, a titanium source, water and isopropanol to obtain a titanium silicalose sol;

[0026] (2) adding the compound represented by formula (I) to the titanium silicalose sol, and subjecting the obtained mixture to hydrothermal crystallization and calcination;

[0027]

[0028] Wherein, i is an integer of 0-10; R1, R2 and R3 are each independently selected from a C1-C6 alkyl group.

[0029] In the present invention, the C1-C6 alkyl group refers to an alkyl group having 1 to 6 carbon atoms in total, for example, it can be one of methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, tert-butyl, n-pentyl and n-hexyl.

[0030] In the present invention, the number of methylene groups between the phenyl group and the methyl group is 0-10; in some preferred embodiments of the present invention, i is an integer of 1-5, for example, 1, 2, 3, 4 or 5; that is, the number of methylene groups between the phenyl group and the methyl group is 1-5.

[0031] In some preferred embodiments of the present invention, R1, R2 and R3 are each independently selected from a C1-C3 alkyl group, and the C1-C3 alkyl group may be a methyl group, an ethyl group, a n-propyl group or an isopropyl group. Preferably, R1, R2 and R3 are each independently selected from a methyl group, an ethyl group or an n-propyl group. In the present invention, R1, R2 and R3 may be the same or different. Preferably, R1, R2 and R3 are the same.

[0032] In the present invention, a compound represented by formula (I) is used as a silanization agent, one end of which is a phenyl composite alkyl group. During the hydrothermal crystallization process, the phenyl group, as a powerful supporting layer structure, can play a supporting role during the hydrolysis and condensation of the titanium silical sol, so that the molecular sieve crystal has a microporous structure and a mesoporous structure; at the same time, the flexible alkyl group can fine-tune the mesoporous structure obtained by the supporting layer, so that the size of the mesoporous channels is relatively concentrated; the multi-level pore titanium silicalite prepared by this method can selectively oxidize monoolefins into alkylene oxides during the catalytic oxidation of monoolefins, and the reaction effect is significantly improved.

[0033] According to the present invention, if the amount of the silanization agent (the compound shown in formula (I)) is too high, the crystallization performance of the titanium silical sol will deteriorate; if the amount of the silanization agent (the compound shown in formula (I)) is too low, the specific surface area of ​​the obtained titanium silicalite will be reduced, and the mesoporous structure of the titanium silicalite will also change, affecting the mass transfer effect and further affecting its catalytic oxidation activity of monoolefins; under preferred conditions, in step (1), the silicon source is calculated as SiO2, and the molar ratio of the silicon source to the compound shown in formula (I) is 1:(0.01-0.3), preferably 1:(0.01-0.2); more preferably 1:(0.05-0.12).

[0034] In some preferred embodiments of the present invention, the silicon source is calculated as SiO2, the alkaline template is calculated as N when it contains nitrogen, and the alkaline template is calculated as OH when it does not contain nitrogen. - The molar ratio of the silicon source, the alkaline template and water is 1:(0.05-0.4):(5-40); preferably 1:(0.1-0.3):(5-25).

[0035] According to the present invention, under preferred conditions, the silicon source is selected from at least one of tetramethyl silicate, tetraethyl silicate, tetrapropyl silicate, tetrabutyl silicate, silica gel, white carbon black and silica sol;

[0036] According to the present invention, under preferred conditions, the alkaline template is selected from at least one of quaternary ammonium bases, aliphatic amines and aliphatic alcohol amines, preferably at least one of tetramethylammonium hydroxide, tetraethylammonium hydroxide, tetrapropylammonium hydroxide and tetrabutylammonium hydroxide.

[0037] In some preferred embodiments of the present invention, the silicon source is calculated as SiO2, the titanium source is calculated as TiO2, and the molar ratio of the silicon source, the titanium source and isopropanol is 1:(0.001-0.04):(0.1-10), preferably 1:(0.005-0.025):(0.1-5).

[0038] According to the present invention, under preferred conditions, the titanium source is selected from an organic titanium source and / or an inorganic titanium source; further preferably, the titanium source is selected from at least one of titanium tetrachloride, titanium sulfate, titanium nitrate, tetraethyl titanate, tetrapropyl titanate and tetrabutyl titanate.

[0039] According to the present invention, under preferred conditions, step (1) further comprises: first stirring and mixing the silicon source, the alkaline template and water to obtain a mixed system; then dropwise adding a mixed solution of the titanium source and isopropanol into the mixed system for a second stirring to obtain a mixed solution.

[0040] In the present invention, the droplet acceleration rate of the mixed solution is preferably 0.01-0.5 mL / min; more preferably 0.1-0.5 mL / min.

[0041] In the present invention, preferably, the first stirring time is 0.1-2h.

[0042] In the present invention, preferably, the second stirring time is 0.5-6h, preferably 0.5-3h.

[0043] In the present invention, preferably, step (1) further comprises: driving out alcohol from the mixed solution; driving out alcohol can remove alcohol generated by hydrolysis of silicon source and titanium source, and in the present invention, preferably, azeotropic distillation is used to remove alcohol generated in the system, and water lost by azeotropic distillation is supplemented during the driving out alcohol process to ensure that the ratio of each substance in the titanium silica sol meets the above requirements; preferably, the conditions for driving out alcohol include: temperature of 30-100°C and time of 2-10h; preferably temperature of 40-90°C and time of 4-10h.

[0044] According to the present invention, in order to make the silanization agent uniformly dispersed in the titanium silica sol; under preferred conditions, step (1) also includes: adding the compound represented by formula (I) to the titanium silica sol and performing a third stirring for 0.1-24h, preferably the third stirring time is 0.5-10h, more preferably 1-5h.

[0045] In the present invention, the nucleation and growth rates of the molecular sieve at low temperature can be controlled by rapidly heating, thereby obtaining molecular sieve particles with smaller sizes; under preferred conditions, in step (2), the conditions for hydrothermal crystallization include: heating the mixture to 50-200°C within 0.1-1h, and then performing hydrothermal crystallization at 50-200°C for 10-100h; preferably, performing hydrothermal crystallization at a temperature of 100-200°C for 20-80h; further preferably, the heating time is 0.3-1h; more preferably, the conditions for hydrothermal crystallization include: a temperature of 120-180°C and a time of 20-80h; under the above preferred conditions, the crystallinity, specific surface area and pore volume of the molecular sieve can be balanced; and a molecular sieve with specific crystallinity, specific surface area and pore volume can be prepared.

[0046] The present invention has no particular limitation on the pressure of hydrothermal crystallization, which may be the autogenous pressure of the crystallization system.

[0047] According to the present invention, under preferred conditions, the method further comprises: washing, filtering and drying the product obtained by hydrothermal crystallization; wherein the washing, filtering and drying processes can be known to those skilled in the art. Exemplarily, the washing temperature can be 20-50°C, the washing solvent can be water, and the amount of the washing solvent is 1-20 times the mass of the crystallized product; the drying conditions can be: the temperature is 40-150°C and the time is 0.5-24h.

[0048] In some preferred embodiments of the present invention, the calcination conditions include: a temperature of 400-800° C. and a time of 1-15 h; preferably a temperature of 500-600° C. and a time of 4-10 h.

[0049] The third aspect of the present invention provides a multi-level pore titanium silicon molecular sieve prepared according to the method described in the second aspect.

[0050] Preferably, the mesopore diameter of the multi-level pore titanium silicon molecular sieve is 5-10 nm, and the specific surface area is 500-650 m 2 / g, with a total pore volume of 0.45-0.8cm 3 / g, with an external surface area of ​​120-300m 2 / g, micropore diameter is 0.1-2nm; micropore volume is 0.12-0.2cm 3 / g, the particle size of the molecular sieve particles is 100-250nm, and the crystallinity of the molecular sieve is ≥50%; further preferably, in the infrared spectrum of the multi-level pore titanium silicon molecular sieve, the wave number is 960cm -1 Peak area and wave number 800cm -1 The ratio of the peak area of 960 / I 800 ) is 0.7-2.

[0051] According to the present invention, under preferred conditions, the molar ratio of titanium to silicon in the multi-level porous titanium silicon molecular sieve is 0.001-0.04:1; preferably 0.005-0.025:1.

[0052] Further preferably, the titanium silicalite has high activity in catalyzing the epoxidation of monoolefins. In the catalytic epoxidation reaction of monoolefins, the conversion rate of monoolefins is increased to more than 90%, and the selectivity of monoolefin epoxidation products is increased to more than 90%.

[0053] The fourth aspect of the present invention provides a method for epoxidation of a monoolefin, the method comprising: contacting a monoolefin and a peroxide for reaction in the presence of a catalyst, wherein the catalyst comprises the multi-level porous titanium silicon molecular sieve described in the first aspect or the third aspect.

[0054] According to the present invention, under preferred conditions, the monoolefin is selected from C3-C 15 Monoolefins, preferably C5-C 10 further preferably, the monoolefin is selected from at least one of 1-octene, cyclohexene and styrene.

[0055] According to the present invention, under preferred conditions, the peroxide is selected from at least one of tert-butyl hydroperoxide, cyclohexyl hydroperoxide, isopropyl hydroperoxide, cumene hydroperoxide, hydrogen peroxide, sodium percarbonate and sodium perborate.

[0056] According to the present invention, under preferred conditions, the reaction conditions include: the weight ratio of the catalyst to the monoolefin is 1:(1-20); the molar ratio of the monoolefin to the peroxide is 1:(0.1-10); further preferably, the reaction conditions include: temperature of 40-100°C and time of 1-8h.

[0057] In the present invention, the catalyst may be a full molecular sieve or may contain a carrier; when used for catalyzing the epoxidation of monoolefins, the multi-level pore titanium silicon molecular sieve particles are directly used as the catalyst.

[0058] According to a particularly preferred embodiment of the present invention, the method for preparing a multi-level porous titanium silicon molecular sieve comprises:

[0059] (1) mixing a silicon source, an alkaline template and water in a molar ratio of 1:(0.1-0.3):(5-25), stirring for a first time at room temperature for 0.1-2 hours, then adding a mixed solution of a titanium source and isopropanol dropwise to the mixed system at a rate of 0.1-0.5 mL / min, stirring for a second time for 0.5-3 hours, and obtaining a mixed solution; wherein the molar ratio of the silicon source, the titanium source and isopropanol is 1:(0.005-0.025):(0.1-5);

[0060] Then, the mixed system is subjected to alcohol removal to obtain titanium silicalose; the temperature of the alcohol removal is 40-90° C. and the time is 4-10 hours;

[0061] (2) adding the compound represented by formula (I) to the titanium silicalose, performing a third stirring for 1-2 hours, and performing hydrothermal crystallization and calcination on the obtained mixture; wherein the molar ratio of the silicon source to the compound represented by formula (I) is 1:(0.01-0.2), and the crystallization conditions are: heating the mixture to 120-180° C. within 0.3-1 hour, and then performing hydrothermal crystallization at 120-180° C. for 20-80 hours;

[0062]

[0063] Wherein, i is an integer of 1-5; R1, R2 and R3 are the same and are selected from methyl, ethyl, n-propyl or isopropyl.

[0064] The present invention will be described in detail below by way of examples. In the following examples, room temperature refers to 25±5°C.

[0065] In the following examples and comparative examples, the X-ray diffraction (XRD) crystal phase diagram of the samples was measured on a Siemens D5005 X-ray diffractometer, the ray source was Cu Kα, the tube voltage was 40 kV, the tube current was 40 mA, the scanning speed was 0.5° / min, and the scanning range was 2θ=5°-35°;

[0066] According to the XRD spectrum, the crystallinity was obtained by fitting using BRUKER's software eva;

[0067] The UV-Vis spectra (UV-Vis) of the samples were obtained by Agilent Cary 300 UV spectrophotometer with a wavelength interval of 3 nm and a scanning range of 190-800 nm;

[0068] The surface area and specific surface area were obtained by measuring the static N2 adsorption-desorption curve of the sample at liquid nitrogen temperature (77.4K) using Micromeritics' ASAP2405J static nitrogen adsorption instrument and then performing BET fitting on the adsorption curve.

[0069] The pore volume was determined according to the method described in RIPP 151-90 in "Analytical Methods in Petrochemical Industry" compiled by Yang Cuiding et al. (Science Press, first edition, published in September 1990);

[0070] The pore size distribution was calculated according to the BJH formula;

[0071] The particle size of the molecular sieves was measured by a JEOL JEM-2100 transmission electron microscope (TEM).

[0072] In the following examples, the chemical structural formulas of the silanization agents used are shown in Table 1; wherein Compound 1, Compound 2 and Compound 3 are all commercially available.

[0073] Table 1

[0074]

[0075]

[0076] Example 1

[0077] (1) white carbon black, tetrabutylammonium hydroxide and water are first stirred and mixed at room temperature for 0.5 h to obtain a mixed system, and during the stirring process, a mixed solution of titanium tetrachloride and isopropanol is added dropwise to the mixed system at a rate of 0.5 mL / min, and a second stirring is performed for 1 h to obtain a mixed solution; white carbon black is calculated as SiO2, tetrabutylammonium hydroxide is calculated as N, titanium tetrachloride is calculated as TiO2, and the molar ratio of white carbon black, tetrabutylammonium hydroxide and water is 1:0.15:20; the molar ratio of white carbon black, titanium tetrachloride and isopropanol is 1:0.005:5;

[0078] Then, the mixed solution was subjected to alcoholization at 80°C for 5 hours to obtain titanium silicalose;

[0079] (2) adding compound (1) to titanium silicalose, and stirring for a third time at room temperature for 1 hour to obtain a mixture, wherein the molar ratio of compound (1) to white carbon black is 0.05:1;

[0080] (3) heating the mixture to 120° C. for 0.5 h, and performing hydrothermal crystallization at 120° C. for 72 h to obtain a crystallized product; the crystallized product was sequentially rinsed with water, filtered, and dried at 120° C. for 2 h;

[0081] The dried product was calcined at 550°C for 6 hours to obtain titanium silicon molecular sieve;

[0082] The pore size distribution of the titanium silicate molecular sieve obtained in this example is as follows: Figure 1 As shown, the N2 adsorption and desorption curve is as follows Figure 2 shown; from Figure 1 and Figure 2 It can be seen that the titanium silicon molecular sieve obtained in this embodiment contains both a microporous structure and a mesoporous structure with a pore size of about 8 nm;

[0083] The TEM image of the titanium silicon molecular sieve obtained in this example is as follows: Figure 3 As shown, from Figure 3 It can be seen that the particle size of the titanium silicon molecular sieve obtained in this embodiment is about 100-200nm;

[0084] The XRD spectrum of the titanium silicon molecular sieve obtained in this example is as follows: Figure 4 As shown, from Figure 4 It can be seen that the titanium silicon molecular sieve obtained in this embodiment has an MFI structure and good crystallization performance;

[0085] The physical properties of the titanium silicate molecular sieve obtained in this example are shown in Table 3.

[0086] Embodiment 2-20

[0087] Titanium silicate molecular sieve was prepared according to the method of Example 1. The proportion and synthesis conditions are shown in Table 2. The physical properties and catalytic performance of the prepared molecular sieve are shown in Table 3.

[0088] Comparative Example 1

[0089] Titanium silicon molecular sieve was prepared according to the method of Example 1 of CN106145151B, and the specific method is as follows:

[0090] Ethyl orthosilicate, tetrapropylammonium hydroxide, tetrabutyl titanate and deionized water were mixed to obtain a mixture with a molar ratio of SiO2: structure directing agent: TiO2: H2O = 1: 0.2: 0.025: 50. Then, quaternized cellulose and N-phenyl-3-aminopropyltrimethoxysilane were added to the titanium silicate molecular sieve precursor gel mixture at a molar ratio of SiO2 to silanization agent of 1: 0.1 and a weight ratio of SiO2 to natural polymer compound of 1: 0.1. After stirring evenly, the titanium silicate molecular sieve precursor treated with the silanization agent and modified natural polymer compound was transferred to a pressure-resistant stainless steel reactor; heated to 170°C under stirring and crystallized under autogenous pressure for 24 hours. After the stainless steel pressure-resistant reactor was cooled to room temperature, the uncalcined titanium silicate molecular sieve was recovered, dried at 110°C for 6 hours, and then calcined at 550°C for 4 hours to obtain the multi-level porous titanium silicate molecular sieve TS-1. The pore size distribution diagram is as follows Figure 5 The product characteristics are shown in Table 3.

[0091] Comparative Examples 2-6

[0092] Titanium silicate molecular sieve was prepared according to the method of Example 1. The proportion and synthesis conditions are shown in Table 2. The physical properties and catalytic performance of the prepared molecular sieve are shown in Table 3.

[0093] Comparative Example 7

[0094] Titanium silicate molecular sieve was prepared according to the method of Example 1, except that the silanization agent was phenyltriethoxysilane (Compound 4), whose structural formula is shown in Formula (II), whose proportion and synthesis conditions are shown in Table 2, and the physical properties and catalytic performance of the prepared molecular sieve are shown in Table 3;

[0095]

[0096] Comparative Example 8

[0097] Titanium silicate molecular sieve was prepared according to the method of Example 1, except that the structural formula of the silanization agent (Compound 5) is as shown in Formula (III), the ratio and synthesis conditions thereof are shown in Table 2, and the physical properties and catalytic performance of the prepared molecular sieve are shown in Table 3;

[0098]

[0099] Comparative Example 9

[0100] Titanium silicate molecular sieve was prepared according to the method of Example 1, except that the structural formula of the silanization agent (Compound 6) is shown in Formula (IV), the ratio and synthesis conditions thereof are shown in Table 2, and the physical properties and catalytic performance of the prepared molecular sieve are shown in Table 3.

[0101]

[0102] Test Case

[0103] This test example illustrates the reaction effect of the molecular sieves prepared by Examples 1-20 and Comparative Examples 1-9 provided by the present invention for the epoxidation reaction of 1-octene to prepare 1,2-epoxyoctane. The reagents used in this test example are all commercially available chemically pure reagents. The concentration of each substance after the reaction is quantitatively analyzed using gas chromatography. The instrument used is a 6890 gas chromatograph produced by Agilent; the analytical chromatographic column used is an HP-5 capillary chromatographic column and a hydrogen flame ionization detector. The component concentration is quantified using the external standard method. First, the peak area of ​​each component is measured, the component concentration is checked through the standard working curve, and the selectivity and other indicators of the corresponding product are calculated.

[0104] In the test example, the 1-octene conversion rate and the 1,2-octane oxide selectivity were calculated according to the following formulas:

[0105] 1-octene conversion rate % = (1-1-octene moles remaining after reaction / 1-octene moles added before reaction) × 100%

[0106] 1,2-Octene oxide selectivity % = number of moles of 1,2-octene oxide after reaction / (number of moles of 1-octene added before reaction - number of moles of 1-octene remaining after reaction) × 100%

[0107] The titanium silicon molecular sieves prepared in the above Examples 1-20 and Comparative Examples 1-9 were respectively used as catalysts, and added into a three-necked flask according to the mass ratio of catalyst, 1-octene and solvent acetonitrile of 1:20:100, and mixed evenly under magnetic stirring. After the temperature was raised to 50° C. by electric heating, an aqueous hydrogen peroxide solution (30% by weight) was added to the above mixture, the molar ratio of 1-octene to hydrogen peroxide was 1:1, the reaction temperature was maintained at 50° C., the reaction time was 6 h, and samples were taken for chromatographic analysis. The reaction results are shown in Table 3.

[0108] It can be seen from the results in Table 3 that the titanium silicalite molecular sieve of the present invention has high 1-octene epoxidation activity. In the catalytic 1-octene epoxidation reaction, the conversion rate of 1-octene is increased to 98%, and the selectivity of 1,2-octane oxide is increased to 97%.

[0109] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

[0110]

[0111]

[0112]

Claims

1. A multi-level pore titanium silicon molecular sieve, characterized in that: The mesopore diameter of the multi-level pore titanium silicon molecular sieve is 5-10nm, and the specific surface area is 500-650m 2 / g, with a total pore volume of 0.45-0.8cm 3 / g, with an external surface area of ​​120-300m 2 / g, micropore diameter is 0.1-2nm, micropore volume is 0.12-0.2cm 3 / g, the particle size of the molecular sieve particles is 100-250nm, and the crystallinity of the molecular sieve is ≥50%; In the infrared spectrum of the multi-level porous titanium silicon molecular sieve, the wave number is 960cm -1 The peak area and wave number of 800cm -1 The ratio of the peak areas is 0.7-2.

2. The multi-level pore titanium silicon molecular sieve according to claim 1, wherein: The molar ratio of titanium to silicon in the multi-level porous titanium silicon molecular sieve is 0.001-0.04:

1.

3. The multi-level pore titanium silicon molecular sieve according to claim 2, wherein: The molar ratio of titanium to silicon in the multi-level porous titanium silicon molecular sieve is 0.005-0.025:

1.

4. A method for preparing a multi-level porous titanium silicon molecular sieve, characterized in that: The method comprises: (1) mixing a silicon source, an alkaline template, a titanium source, water and isopropanol to obtain a titanium silicalose sol; (2) adding the compound represented by formula (I) to the titanium silicalose sol, and subjecting the obtained mixture to hydrothermal crystallization and calcination; wherein i is an integer from 0 to 10; R1, R2 and R3 are each independently selected from a C1-C6 alkyl group; The silicon source is calculated as SiO2, and the molar ratio of the silicon source to the compound represented by formula (I) is 1:(0.01-0.3); The silicon source is calculated as SiO2, the alkaline template is calculated as N when it contains nitrogen, and as OH when it does not contain nitrogen. - The titanium source is calculated as TiO2, The molar ratio of the silicon source, the alkaline template and water is 1:(0.05-0.4):(5-40); The molar ratio of the silicon source, the titanium source and isopropanol is 1:(0.001-0.04):(0.1-10); In step (2), the hydrothermal crystallization conditions include: heating the mixture to 50-200° C. within 0.1-1 h, and then crystallizing at 50-200° C. for 10-100 h.

5. The method according to claim 4, wherein: i is an integer from 1 to 5.

6. The method according to claim 4, wherein: R1, R2 and R3 are each independently selected from methyl, ethyl or propyl.

7. The method according to claim 4, wherein: The silicon source is calculated as SiO2, and the molar ratio of the silicon source to the compound represented by formula (I) is 1:(0.01-0.2).

8. The method according to any one of claims 4 to 7, wherein: The silicon source is calculated as SiO2, the alkaline template is calculated as N when it contains nitrogen, and as OH when it does not contain nitrogen. - The titanium source is calculated as TiO2, The molar ratio of the silicon source, the alkaline template and water is 1:(0.1-0.3):(5-25); The molar ratio of the silicon source, the titanium source and isopropanol is 1:(0.005-0.025):(0.1-5).

9. The method according to any one of claims 4 to 7, wherein: The silicon source is selected from at least one of tetramethyl silicate, tetraethyl silicate, tetrapropyl silicate, tetrabutyl silicate, silica gel, white carbon black and silica sol.

10. The method according to any one of claims 4 to 7, wherein: The alkaline template agent is selected from at least one of quaternary ammonium base, aliphatic amine and aliphatic alcohol amine.

11. The method according to claim 10, wherein: The alkaline template agent is selected from at least one of tetramethylammonium hydroxide, tetraethylammonium hydroxide, tetrapropylammonium hydroxide and tetrabutylammonium hydroxide.

12. The method according to any one of claims 4 to 7, wherein: The titanium source is selected from an organic titanium source and / or an inorganic titanium source.

13. The method according to claim 12, wherein: The titanium source is selected from at least one of titanium tetrachloride, titanium sulfate, titanium nitrate, tetraethyl titanate, tetrapropyl titanate and tetrabutyl titanate.

14. The method according to any one of claims 4 to 7, wherein: Step (1) also includes: stirring and mixing a silicon source, an alkaline template, and water to obtain a mixed system; and then dropwise adding a mixed solution of a titanium source and isopropanol into the mixed system to obtain a mixed solution.

15. The method according to claim 14, wherein: The droplet acceleration rate of the mixed solution is 0.01-0.5 mL / min.

16. The method according to claim 14, wherein: Step (1) also includes: removing alcohol from the mixed solution.

17. The method according to claim 16, wherein: The conditions for driving out the alcohol include: temperature of 30-100° C. and time of 2-10 h.

18. The method according to claim 17, wherein: The conditions for driving out the alcohol include: temperature of 40-90° C. and time of 4-10 h.

19. The method according to any one of claims 4 to 7, wherein: In step (2), the hydrothermal crystallization conditions include: performing crystallization at a temperature of 100-200° C. for 20-80 hours.

20. The method according to any one of claims 4 to 7, wherein: The calcination conditions include: temperature of 400-800° C. and time of 1-15 hours.

21. A hierarchical pore titanium silicon molecular sieve prepared according to the method according to any one of claims 4 to 20.

22. The titanium silicalite molecular sieve according to claim 21, wherein: The mesopore diameter of the multi-level pore titanium silicon molecular sieve is 5-10nm, and the specific surface area is 500-650m 2 / g, with a total pore volume of 0.45-0.8cm 3 / g, with an external surface area of ​​120-300m 2 / g, micropore diameter is 0.1-2nm; micropore volume is 0.12-0.2cm 3 / g, the particle size of the molecular sieve particles is 100-250nm, and the crystallinity of the molecular sieve is ≥50%.

23. The titanium silicalite molecular sieve according to claim 21, wherein: The molar ratio of titanium to silicon in the multi-level porous titanium silicon molecular sieve is 0.001-0.04:

1.

24. The titanium silicon molecular sieve according to claim 23, wherein: The molar ratio of titanium to silicon in the multi-level porous titanium silicon molecular sieve is 0.005-0.025:

1.

25. The titanium silicalite molecular sieve according to claim 21, wherein: In the infrared spectrum of the multi-level porous titanium silicon molecular sieve, the wave number is 960cm -1 Peak area and wave number 800cm -1 The ratio of the peak areas is 0.7-2.

26. A method for the epoxidation of a monoolefin, the method comprising: In the presence of a catalyst, a monoolefin and a peroxide are contacted to react, wherein the catalyst comprises the multi-level porous titanium silicon molecular sieve according to claim 1, 2, 3, 21, 22, 23, 24 or 25.

27. The method according to claim 26, wherein: The monoolefin is selected from C3-C 15 of monoolefins.

28. The method according to claim 27, wherein: The monoolefin is selected from C5-C 10 of monoolefins.

29. The method according to claim 28, wherein: The monoolefin is selected from at least one of 1-octene, cyclohexene and styrene.

30. The method of claim 26, wherein: The peroxide is selected from at least one of tert-butyl hydroperoxide, cyclohexyl hydroperoxide, isopropyl hydroperoxide, cumene hydroperoxide, hydrogen peroxide, sodium percarbonate and sodium perborate.

31. The method of claim 26, wherein: The reaction conditions include: the weight ratio of the catalyst to the monoolefin is 1:(1-30); the molar ratio of the monoolefin to the peroxide is 1:(0.1-10).

32. The method of claim 26, wherein: The reaction conditions include: temperature of 40-100° C. and time of 1-8 h.

Citation Information

Patent Citations

  • A hierarchical porous titanium-silicon molecular sieve and its synthesis method

    CN106145151B

  • Hierarchical porous titanium-silicon molecular sieve as well as preparation method thereof and olefin epoxidation method

    CN108726528A

  • Interior surface coating structure mesoporous titanium silicate molecular sieve material and preparation method and use thereof

    CN101417809A

  • Method for preparing mesoporous titanium silicate molecular sieve

    CN101456562A

  • Method for preparing p-benzoquinone

    CN107400051A