A production process of yak down / yak hair / comfortable stretch yarn mixed flakes

By adding water, kneading, removing impurities and combing the washed yak down to form two fine hairs, and mixing it with elastic silk to prepare flakes, it solves the problem of using scraps and improves the overall utilization efficiency of yak down. Preparation The flakes have good warmth retention and environmental protection.

CN116334835BActive Publication Date: 2024-10-29ELEGANT PROSPER ZHEJIANG GARMENT
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202211722085.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-30
Publication Date
2024-10-29
Estimated Expiration
2042-12-30

AI Technical Summary

Technical Problem

The fineness of the scraps produced during the carding process of yak down is relatively thick, which increases the difficulty of spinning and causes many ends to be broken during processing, affecting the yarn's dryness and strength. How to effectively utilize these scraps becomes a problem.

Method used

The washed yak down velvet is added with water, and the hair is opened, impurities are removed and carded to form two fine hairs. It is mixed with elastic silk and opened and carded according to the weight ratio to form a mixed raw material, which is then prepared into floc through a carding machine and a laying machine. The fiber web is formed into mixed flakes through needle punching equipment, and is finally cut and rolled.

Benefits of technology

Effective utilization of secondary fine hair improves the overall utilization efficiency of washed yak down and reduces the waste of natural resources. The prepared flakes have good warmth retention and environmental protection.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004030010970000101
    Figure BDA0004030010970000101
Patent Text Reader

Abstract

The present invention relates to a production process of a yak down / yak hair / comfortable elastic yarn mixed flakes, comprising the following steps: preparation of two fine hairs, mixing, combing, web laying, needling, slitting and winding. The two fine hairs are formed by adding water, opening, removing impurities and combing the original yak down; the average fineness of the two fine hairs is 24-29 μm, the length is 30-37 mm, and it contains 50-70% yak hair, and the rest is yak down; the gram weight of the mixed flakes is 60-500 grams per square meter. The flakes formed by needling the two fine hairs left over in the combing process of yak down and the comfortable elastic yarn can effectively utilize the two fine hairs, improve the overall utilization efficiency of the washed yak down, reduce the waste of natural resources, and make the prepared flakes have good warmth retention, and are more environmentally friendly than flakes made of purified fiber.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of flake production, in particular to a production process of yak down / yak hair / comfortable stretch yarn mixed flakes. Background Art

[0002] Yak wool is a rare natural high-grade protein textile fiber in the world. It is soft, smooth, elastic, and not easy to shrink. It is a high-grade raw material for the textile industry. The average fineness of yak wool is 19.5μm. However, the output of yak wool is relatively small and is usually used for high-grade fabrics. In the process of combing and preparing yak wool for textile use from the washed yak wool, some scraps will appear. The fineness is coarser than the diameter of yak wool, which is quite different from the diameter of yak wool used for textiles. This will increase the difficulty of spinning, cause more breakages during processing, and affect the yarn dryness and strength. How to use the scraps left over from the combing of yak wool has become a problem to be solved. Summary of the invention

[0003] In order to solve the above technical problems, the purpose of the present invention is to provide a production process of yak down / yak hair / comfortable stretch yarn mixed flakes.

[0004] To solve the above technical problems, the purpose of the present invention is achieved as follows:

[0005] The present invention relates to a production process of yak down / yak hair / comfortable stretch yarn mixed flakes, comprising the following steps:

[0006] S1. Preparation of fine wool: washing yak wool and forming fine wool by adding water, loosening, removing impurities and combing; the fine wool has an average fineness of 24-29 μm, a length of 30-37 mm, contains 50-70% yak wool, and the rest is yak wool; the fineness of yak wool is less than or equal to 35 μm, and the fineness of yak hair is greater than 35 μm;

[0007] S2, mixed fleece: the two fine wools prepared in the previous step and the stretch yarns are opened and combed according to a weight ratio to form a mixed raw material;

[0008] S3, combing: the mixed raw material prepared in the previous step is conveyed to the combing machine through the down feeding machine to be combed into a mixed fiber web and sent to the next process;

[0009] S4, web laying: the mixed fiber web prepared in the previous step is passed through a web laying machine to form a flocculent fiber web with a certain thickness;

[0010] S5, acupuncture: feeding the flocculent fiber web into acupuncture equipment, and the needles repeatedly penetrate the flocculent fiber web in a vertical direction, so that the fibers are entangled with each other to form mixed floccules, and the gram weight of the mixed floccules is 60-500 grams per square meter;

[0011] S6, slitting and rolling: the mixed flakes are slitting and rolling up by slitting and rolling equipment to form flake rolls with specified width and length.

[0012] Based on the above scheme and as a preferred scheme of the above scheme: in step S1, adding water means adding water to the washed yak wool so that the moisture regain of the washed yak wool is maintained at about 30%, and then standing for 24 hours;

[0013] The specific steps of adding water are as follows: first spread a layer of washed yak wool on the clean workshop floor, spray tap water by spraying method, then spread another layer of washed yak wool, spray tap water again, and repeat this process, spread 4 layers of washed yak wool in total, each layer is 20-25cm high, and the weight of the sprayed tap water accounts for 15-20% of the washed yak wool.

[0014] On the basis of the above scheme and as a preferred scheme of the above scheme: in step S1, the wool opening adopts a single cylinder opening machine, the washed yak wool after absorbing water is manually cut and the washed yak wool layer is put into the wool bucket, the washed yak wool is transported to the wool feeding curtain by the air flow through the air duct, the wool feeding curtain transports the washed yak wool to the cylinder through the working roller, and then outputs it through the doffer, and finally is rolled into the wool bin by the fan through the pipeline, and the speed of the cylinder is adjusted to 100r / min.

[0015] On the basis of the above scheme and as a preferred scheme of the above scheme: in step S1, the impurity removal is to use an impurity remover to remove impurities from the washed yak wool after wool mixing; the combing is to use a cotton-type single cylinder carding machine to comb the yak wool after impurities removal, and the workshop temperature is controlled at 22-30°C during combing, and the relative humidity is maintained at 60-70%; the card clothing used by the single cylinder carding machine is a 3510 metal card clothing, and the rotation speed of the cylinder is 200r / min; in this step, the feeding curtain and the licker-in rod in the single cylinder carding machine have a gauge of 25 wires, the licker-in rod and the cylinder have a gauge of 10 wires, the cylinder and the upper cover plate have a gauge of 25 wires, the lower funnel has a gauge of 40 wires, and the doffer has a gauge of 10 wires; after combing, the average fineness of the hairless yak wool is detected, and the average fineness is required to be less than 19.5μm, and the coarseness content is controlled within 12%;

[0016] The scraps formed after the combing in the previous step are combed again by a single cylinder carding machine; in this step, the distance between the feeding wool curtain and the licker-in rod in the single cylinder carding machine is 30 threads, the distance between the licker-in rod and the cylinder is 15 threads, the distance between the cylinder and the upper cover plate is 30 threads, the distance between the cylinder and the lower funnel is 45 threads, and the distance between the cylinder and the doffer is 15 threads; the two fine wools formed after combing are required to have an average fineness of 24μm to 29μm, and those greater than 29μm are wool residues.

[0017] On the basis of the above scheme and as a preferred scheme of the above scheme: in step S2, the opening is that the two fine wools and the stretch yarns are mixed and opened by an opening machine according to a weight ratio to form a mixed raw material, and a small amount of moisture regain is added to avoid the phenomenon of wool curling and wool particles in the wool mixing process;

[0018] The mixed raw materials after opening are fed into the wool bucket of the carding machine through the conveying duct of the opener. The mixed raw materials are fed from the wool bucket to the licker-in roller through the roller. The licker-in roller outputs the raw materials through the cylinder, the cover plate, and the doffer, and the chopper falls into the velvet box.

[0019] The process parameters of the carding machine are as follows: roller: 20 rpm; licker-in: 780 rpm; cylinder: 300 rpm; doffer: 15 rpm.

[0020] On the basis of the above scheme and as a preferred scheme of the above scheme: a bottom leakage and a down suction channel are additionally installed below the licker-in roller of the carding machine.

[0021] On the basis of the above scheme and as a preferred scheme of the above scheme: the down feeding machine controls the amount of down stored in the down box of the down feeding machine through photoelectric control, and the vibration plate on the down feeding machine can evenly adjust the speed to control the amount of down fed, and corner nails are provided in the down box to transport the mixed down in the down box to the next process.

[0022] On the basis of the above scheme and as a preferred scheme of the above scheme: in step S3, a double-doffer single-cylinder high-speed carding machine is used, and the mixed fluff delivered by the fluff feeding machine is fed into the feed roller, and the mixed fiber web is formed by the licker-in roller, the cylinder, and the doffer and sent to the next process;

[0023] The cylinder, doffer, working roller and stripping roller of the double doffer single cylinder high-speed carding machine have all been tempered; the card clothing used is Jinlun card clothing;

[0024] The feed rollers are composed of two pairs of rollers wrapped with metal card clothing, wherein the bearing seats and transmission gears of the first pair of feed rollers are nylon parts and have metal detection function, reversing function and automatic stop alarm function.

[0025] On the basis of the above scheme and as a preferred scheme of the above scheme: in step S4, the web laying is to pass the fed mixed fiber web through the transmission curtain, the oblique curtain on the web laying machine through the middle curtain and the ring curtain and repeatedly swing back and forth to lay it flat on the input curtain to form a flocculent fiber web with a certain thickness for use in the next process.

[0026] Based on the above scheme and as a preferred scheme of the above scheme: in step S5, the needling is that the flocculent fiber web fed on the input curtain of the web laying machine is fed into the upper and lower web stripping spindles of the needling machine, and the upper and lower needling plates repeatedly penetrate the flocculent fiber web at high speed in the vertical direction, so that the fibers are entangled with each other to form mixed flakes;

[0027] In step S6, the trimming and winding is performed by a trimming and winding machine, including longitudinal cutting and transverse cutting. The longitudinal cutting uses a cylinder cutter to cut the mixed flakes into a specified width. The transverse cutting refers to cutting the mixed flakes horizontally after the winding reaches a specified number of meters.

[0028] The beneficial effects of the present invention are as follows: the production process of the yak down / yak hair / comfortable elastic silk mixed flakes involved in the present invention adopts the flakes formed by acupuncture of the two fine hairs remaining in the yak down combing process and the comfortable elastic silk, which can effectively utilize the two fine hairs, improve the overall utilization efficiency of the washed yak down, reduce the waste of natural resources, and make the prepared flakes have good warmth retention, and are more environmentally friendly than the flakes made of purified fiber. DETAILED DESCRIPTION

[0029] The present invention is further described below in conjunction with specific embodiments.

[0030] The present invention relates to a production process of yak down / yak hair / comfortable stretch yarn mixed flakes, comprising the following steps: S1 preparation of two fine hairs, S2 mixing of the wool, S3 combing, S4 laying of nets, S5 needling, and S6 slitting and winding.

[0031] In the preparation of the second fine hair in step S1, the second fine hair is formed by adding water to the washed yak wool, loosening the wool, removing impurities and combing; the average fineness of the second fine hair is 24-29 μm, the length is 30-37 mm, and it contains 50-70% yak hair, and the rest is yak wool; the fineness of the yak wool is less than or equal to 35 μm, and the average fineness is 19.5 μm; the fineness of yak hair is greater than 35 μm.

[0032] In this step, adding water means adding water to the washed yak wool so that the moisture regain of the washed yak wool is maintained at about 30%, and then leaving it to stand for 24 hours, so that the yak wool fibers can fully absorb moisture.

[0033] The specific steps of adding water are as follows: first spread a layer of washed yak wool on the clean workshop floor, spray tap water by spraying method, then spread another layer of washed yak wool, spray tap water again, and repeat this process, spread 4 layers of washed yak wool in total, each layer is 20-25cm high, and the weight of the sprayed tap water accounts for 15-20% of the washed yak wool.

[0034] In the conventional spinning process of yak wool, wool oil is added during the spinning process. In the present application, the final product is not yarn but flakes, so the requirements for the fiber are relatively low. Under the premise of ensuring the quality of the final product, in order to reduce pollution and improve the cost performance, tap water is added during the spinning process to keep the yak wool fibers at a certain humidity, reduce the friction coefficient between each other, reduce the damage to the fibers in the subsequent process, prevent the generation of static electricity, and reduce the loss of flying hair and falling chips.

[0035] In step S1, the wool opening adopts a single cylinder opening machine, the washed yak wool after absorbing water is manually cut and the washed yak wool layer is put into the wool bucket, the washed yak wool is transported to the wool feeding curtain by the air flow through the air duct, the wool feeding curtain transports the washed yak wool to the cylinder through the working roller, and then outputs it through the doffer, and finally is rolled into the wool bin through the pipeline by the fan, the speed of the cylinder is adjusted to 100r / min, the speed of the cylinder is slow, which can ensure that the fiber damage is minimized, and no additives are added during the process.

[0036] In step S1, the impurities are removed by using an impurity remover on the washed yak wool after woolening. The washed yak wool contains a lot of impurities and needs to be removed before combing. The domestic B272 impurity remover is used to mainly remove grass clippings, dust, etc.

[0037] In step S1, the combing is to use a cotton-type single-cylinder carding machine to comb the yak wool after impurities are removed. The combing equipment used is a domestic 186 cotton-type single-cylinder carding machine, which is modified and the card clothing used by the equipment is replaced with No. 3510 metal card clothing.

[0038] During combing, the workshop temperature is controlled at 22-30℃, and the relative humidity is maintained at 60-70%; the rotation speed of the cylinder in the single cylinder carding machine is 200r / min. In this step, the distance between the feeding curtain and the pricking rod is 25 threads, the distance between the pricking rod and the cylinder is 10 threads, the distance between the cylinder and the upper cover plate is 25 threads, the distance between the cylinder and the lower funnel is 40 threads, and the distance between the cylinder and the doffer is 10 threads; after combing, the fineness of the yak wool is tested, and the fineness is required to be less than 19.5μm, and the coarseness is controlled within 12%. Generally, 10 combings are performed first, and then the inspection is performed after the combing is completed. If the requirements are not met, combing is performed again until it is qualified. The conventional number of combings is generally between 10-15 times.

[0039] The scraps formed after the first and second combing in the previous step are combed again by a single cylinder carding machine; in this step, the distance between the feeding wool curtain and the licker-in rod is 30 threads, the distance between the licker-in rod and the cylinder is 15 threads, the distance between the cylinder and the upper cover plate is 30 threads, the distance between the cylinder and the lower funnel is 45 threads, and the distance between the cylinder and the doffer is 15 threads; the two fine wools formed after combing are required to have an average fineness between 24μm and 29μm, and those greater than 29μm are wool residues.

[0040] In step S2, the two fine wools prepared in the previous step and the stretch yarns are opened and combed according to the weight ratio to form a mixed raw material. In the present invention, the amount of the two fine wools is 55-65%, and specifically in this embodiment, the two fine wools are 60% and the stretch yarns are 40%.

[0041] In step S2, the opening is to mix and open the two fine hairs and the stretch yarns according to the weight ratio through an opening machine to form a mixed raw material, and add a small amount of moisture regain to avoid the phenomenon of hair curling and hair grains in the process of velvet combination. Adding a small amount of moisture regain means adding a small amount of water to the mixed raw material to increase the water content of the mixed raw material, which is conducive to eliminating the generation of static electricity in the combing process and improving the quality of combing.

[0042] The mixed raw materials after opening are input into the hopper of the carding machine through the air duct of the opener. The mixed raw materials are fed from the hopper to the licker-in roller through the roller. The licker-in roller outputs the raw materials through the cylinder, cover plate and doffer, and the chopper falls into the velvet box to form a waterfall-like fiber web.

[0043] Specifically, the process parameters in the carding machine are: roller: 20 rpm; licker-in: 780 rpm; cylinder: 300 rpm; doffer: 15 rpm.

[0044] Furthermore, a leaky bottom and a down suction channel are installed below the licker-in roller of the carding machine to avoid large losses during the production process.

[0045] In step S3 of combing, the mixed raw material prepared in the previous step is conveyed to a combing machine through a down feeder to be combed into a mixed fiber web and sent to the next process.

[0046] The function of the down feeding process is to evenly transport the mixed raw materials after the down is opened, loosened and combined to the next process. The TU-177 down feeding machine is used. The down feeding machine controls the amount of down in the down box of the down feeding machine by photoelectric control, and the vibration plate on the down feeding machine can evenly adjust the speed to control the amount of down feeding. The down box is provided with corner nails to transport the mixed down in the down box to the next process.

[0047] In this step, the carding machine used is a LCD2-205 double-doffer single-cylinder high-speed carding machine, which is used to card the mixed raw materials delivered by the down feeder to form a fiber web.

[0048] In step S3, a double-doffer single-cylinder high-speed carding machine is used. The mixed raw material delivered by the velvet feeding machine is fed into the feed roller, and the mixed fiber web is formed through the licker-in roller, the cylinder and the doffer and sent to the next process.

[0049] The cylinder, doffer, working roller and stripping roller in the double doffer single cylinder high-speed carding machine have all been quenched and tempered. The quenching and tempering treatment refers to the double heat treatment of quenching and high-temperature tempering of the cylinder, doffer, working roller and stripping roller, the purpose of which is to make the working parts have good comprehensive mechanical properties.

[0050] The card clothing used is gold wheel card clothing. The feed rollers are composed of two pairs of rollers wrapped with metal card clothing, wherein the bearing seat and transmission gear of the first pair of feed rollers are nylon parts, and have metal detection function, reversing function and automatic stop alarm function.

[0051] The mixed fluff after combing by the double-doffer single-cylinder high-speed carding machine has a quality increase of 2 levels, with a loss of 4.5% during the process. The feed roller and doffer discharge are both adjusted by frequency conversion, and can be adjusted in time according to the required weight indicators.

[0052] The gauge of the double doffer single cylinder high-speed carding machine, especially the gauge between the cylinder and the working roller and the doffer, plays a decisive role in the carding efficiency. Among them, the gauge between the cylinder and the doffer is 12mm; the gauge of the five working rollers on the cylinder should be gradually reduced from the first to the fifth working roller, which are 22mm, 19mm, 17mm, 15mm, and 12mm respectively. The order from the first to the fifth is arranged according to the direction of machine operation. This kind of gauge setting is conducive to strengthening the carding effect and reducing fiber damage.

[0053] The speed ratio of the double doffer single cylinder high-speed carding machine can be changed by changing the speed of the working roller or doffer when the cylinder speed is constant. The speed of the cylinder is 380 rpm, the speed of the working roller is 680 rpm, and the speed of the doffer is 35 rpm. The larger the speed ratio, the greater the relative movement speed of the steel needles on the two needle surfaces, the longer the action area between the working roller or doffer needle surface and the cylinder needle surface per unit time, and the more fibers are combed, thereby enhancing the combing efficiency. The size of the speed ratio should take into account the size of the feed load and the state of the mixing. The speed of the cylinder directly affects the level of production.

[0054] In step S4, web laying: the mixed fiber web prepared in the previous step is passed through a TLP-I-380 web laying machine to form a flocculent fiber web with a certain thickness. The web laying is to pass the mixed fiber web fed into the web laying machine through the transmission curtain, the oblique curtain, the middle curtain and the ring curtain, and then repeatedly swing back and forth to lay it flat on the input curtain to form a flocculent fiber web with a certain thickness for use in the next process.

[0055] The main structure of the net machine is composed of horizontal steel, which is thick enough to avoid vibration during operation. The net laying is equipped with a segmented stroke independent frequency conversion control to ensure the quality of the fiber net. The input curtain width is 1800mm, and the width of the netting sheet that can be laid is 1600mm.

[0056] In step S5, the needling is to feed the flocculent fiber web fed on the input curtain of the web laying machine into the upper and lower web stripping spindles of the TLZ-360 type needling machine. Before feeding into the needling machine, non-woven fabrics are added to the upper and lower sides of the flocculent fiber web. The function of the added non-woven fabric is to prevent the floccules from being torn in the subsequent processing. The upper and lower needling plates repeatedly penetrate the flocculent fiber web at high speed in the vertical direction, so that the fibers are entangled with each other to form mixed floccules. The flocculent fiber web is fed into the needling equipment, and the needles repeatedly penetrate the flocculent fiber web in the vertical direction, so that most of its fibers are formed into fiber bundles, and the fibers are irregularly tightened with each other, so that the flocculent sheet is qualitatively formed into a finished flocculent product as a whole, forming a mixed flocculent; the gram weight of the mixed flocculent is 60-500 grams per square meter. After testing, some areas of the surface of the flocculent below 60 grams / square meter are uneven and transparent, and the flocculent needle-punched panel above 500 grams / square meter will be partially broken due to the resistance of the velvet product.

[0057] In step S6, slitting and rolling: the mixed flakes are slitting and rolling up by using slitting and rolling equipment to form flake rolls with specified width and length.

[0058] The trimming and winding is performed by using a TLC-350 trimming and winding machine, including longitudinal cutting and transverse cutting. The longitudinal cutting uses a cylinder cutter to cut the mixed flocs to a specified width, and the transverse cutting refers to cutting the mixed flocs horizontally after the winding reaches a specified number of meters. The longitudinal cutting refers to cutting along the length direction of the mixed flocs, while the transverse cutting refers to cutting along the width direction of the mixed flocs, which is perpendicular to the longitudinal cutting direction.

[0059] The gram weight of the yak wool / yak hair / comfortable elastic silk mixed floccules prepared in the present invention is 100 grams per square meter. In this embodiment, the content of yak hair in the two fine hairs used is 60%, and the content of yak wool is 40%. The yak wool / yak hair / comfortable elastic silk mixed floccules, camel hair and Thinsulate cotton prepared in this embodiment are provided with a layer of 25 grams per square meter of non-woven fabric on both sides of the three kinds of floccules, and then a layer of fabric is sewn on both sides. And the fabrics sewn on the three kinds of floccules are the same.

[0060] The thermal insulation test was carried out in accordance with GB / T35762-2017, and the test results are as follows:

[0061]

[0062] It can be seen from the above table that the yak down / yak hair / comfortable stretch silk mixed flakes prepared by the present invention are better than camel hair in terms of thermal insulation, and have similar thermal insulation performance to Thinsulate flakes, but more than half of them are natural fibers, which are more environmentally friendly, and because the two fine hairs used are the waste materials in the preparation process of yak down, their prices are also very affordable, close to Thinsulate cotton.

[0063] The preferred specific embodiments of the present invention are described in detail above. It should be understood that a person skilled in the art can make many modifications and changes based on the concept of the present invention without creative work. Therefore, any technical solution that can be obtained by a person skilled in the art through logical analysis, reasoning or limited experiments based on the concept of the present invention on the basis of the prior art should be within the scope of protection determined by the claims.

Claims

1. A production process of yak down / yak hair / comfortable stretch yarn mixed flakes, It is characterized in that The steps include: S1. Preparation of two fine hairs: washing yak wool and then adding water, loosening, removing impurities and combing to form two fine hairs; the average fineness of the two fine hairs is 24-29 μm, the length is 30-37 mm, and the content is 50-70% of yak hair, and the rest is yak wool; the fineness of the yak wool is less than or equal to 35 μm, and the fineness of the yak hair is greater than 35 μm; S2, mixed fleece: the two fine wools prepared in the previous step and the stretch yarns are opened and combed according to a weight ratio to form a mixed raw material; S3, combing: the mixed raw material prepared in the previous step is conveyed to the combing machine through the down feeding machine to be combed into a mixed fiber web and sent to the next process; S4, web laying: the mixed fiber web prepared in the previous step is passed through a web laying machine to form a flocculent fiber web with a certain thickness; S5, acupuncture: feeding the flocculent fiber web into acupuncture equipment, and the needles repeatedly penetrate the flocculent fiber web in a vertical direction, so that the fibers are entangled with each other to form mixed floccules, and the gram weight of the mixed floccules is 60-500 grams per square meter; S6, slitting and rolling: the mixed flakes are slitting and rolling up by slitting and rolling equipment to form flake rolls with specified width and length; In step S1, adding water means adding water to the washed yak wool so that the moisture regain of the washed yak wool is maintained at about 30%, and then leaving it to stand for 24 hours; The specific steps of adding water are as follows: first spread a layer of washed yak wool on the clean workshop floor, spray tap water by spraying, then spread another layer of washed yak wool, and then spray tap water, repeat this process, spread 4 layers of washed yak wool in total, each layer is 20-25cm high, and the weight of the sprayed tap water accounts for 15-20% of the washed yak wool; In step S1, the wool opening adopts a single cylinder opening machine, the washed yak wool after water absorption is manually cut and the washed yak wool layer is put into the wool bucket, the washed yak wool is transported to the wool feeding curtain by the air flow through the air duct, the wool feeding curtain transports the washed yak wool to the cylinder through the working roller, and then outputs it through the doffer, and finally is rolled into the wool bin by the fan through the pipeline, and the speed of the cylinder is adjusted to 100r / min; In step S1, the impurity removal is to use an impurity remover to remove impurities from the washed yak wool after wool mixing; the combing is to use a cotton-type single-cylinder carding machine to comb the yak wool after impurities removal, the workshop temperature is controlled at 22-30°C during combing, the relative humidity is maintained at 60-70%, the card clothing used by the single-cylinder carding machine is a 3510 metal card clothing, and the rotation speed of the cylinder is 200r / min; in this step, the feeding curtain and the licker-in rod in the single-cylinder carding machine have a gauge of 25 wires, the licker-in rod and the cylinder have a gauge of 10 wires, the cylinder has a gauge of 25 wires and the upper cover plate, a gauge of 40 wires and the lower funnel, and a gauge of 10 wires and the doffer; after combing, the average fineness of the hairless yak wool is detected, and the average fineness is required to be less than 19.5μm, and the coarseness content is controlled within 12%; The scraps formed after the combing in the previous step are combed again by a single cylinder carding machine. In this step, the feeding wool curtain and the licker-in rod are spaced 30 threads apart, the licker-in rod and the cylinder are spaced 15 threads apart, the cylinder and the upper cover are spaced 30 threads apart, the cylinder and the lower funnel are spaced 45 threads apart, and the cylinder and the doffer are spaced 15 threads apart. The scraps formed after combing are two fine wools, and the average fineness is required to be between 24µm and 29μm, and those greater than 29μm are wool residues.

2. The production process of the yak down / yak hair / comfortable stretch yarn mixed flakes according to claim 1, It is characterized in that In step S2, the opening is to mix and open the two fine wools and the stretch yarns according to the weight ratio through an opening machine to form a mixed raw material, and add a small amount of moisture regain to avoid the phenomenon of wool curling and wool particles in the wool mixing process; The mixed raw materials after opening are fed into the wool bucket of the carding machine through the conveying duct of the opener. The mixed raw materials are fed from the wool bucket to the licker-in roller through the roller. The licker-in roller outputs the raw materials through the cylinder, the cover plate, and the doffer, and the chopper falls into the velvet box. The process parameters of the carding machine are: roller: 20 rpm; licker-in: 780 rpm; Cylinder: 300 rpm; Doffer: 15 rpm.

3. The production process of the yak down / yak hair / comfortable stretch yarn mixed flakes according to claim 1, It is characterized in that A leaking bottom and a down suction channel are additionally arranged below the licker-in roller of the carding machine.

4. The production process of the yak down / yak hair / comfortable stretch yarn mixed flakes according to claim 1, It is characterized in that The down feeding machine controls the amount of down stored in the down box in the down feeding machine by photoelectric control, and the vibration plate on the down feeding machine can adjust the speed evenly to control the amount of down feeding. The down box is provided with corner nails for conveying the mixed down in the down box to the next process.

5. The production process of the yak down / yak hair / comfortable stretch yarn mixed flakes according to claim 1, It is characterized in that In step S3, a double-doffer single-cylinder high-speed carding machine is used, and the mixed fluff delivered by the fluff feeding machine is fed into the feed roller, and the mixed fiber web is formed by the licker-in roller, the cylinder, and the doffer and sent to the next process; The cylinder, doffer, working roller and stripping roller of the double doffer single cylinder high-speed carding machine have all been tempered, and the card clothing used is Jinlun card clothing; The feed rollers are composed of two pairs of rollers wrapped with metal card clothing, wherein the bearing seats and transmission gears of the first pair of feed rollers are nylon parts and have metal detection function, reversing function and automatic stop alarm function.

6. The production process of the yak down / yak hair / comfortable stretch yarn mixed flakes according to claim 1, It is characterized in that In step S4, the web laying is to lay the fed mixed fiber web on the input curtain by repeatedly swinging back and forth through the transmission curtain, the oblique curtain, the middle curtain and the ring curtain on the web laying machine to form a flocculent fiber web with a certain thickness for use in the next process.

7. The production process of the yak down / yak hair / comfortable stretch yarn mixed flakes according to claim 1, It is characterized in that In step S5, the needling is to feed the flocculent fiber web fed on the input curtain of the web laying machine into the upper and lower web stripping spindles of the needling machine, and before feeding into the needling machine, non-woven fabrics are added to the upper and lower sides of the flocculent fiber web respectively; The upper and lower needle punching plates repeatedly penetrate the flocculent fiber web at high speed in the vertical direction, causing the fibers to entangle with each other to form mixed flakes; In step S6, the slitting and winding is performed by a trimming and winding machine, including longitudinal slitting and transverse slitting. The longitudinal slitting uses a cylinder cutter to slit the mixed flakes into a specified width. The transverse slitting refers to cutting the mixed flakes horizontally after the winding reaches a specified number of meters.

Citation Information

Patent Citations

  • Technology for loosening and blending cashmere in carding process

    CN106192083A

  • Production process of tensile high-elasticity cashmere wool flakes

    CN109355805A

  • Production method of blended yarns of cashmere fiber and renewable elastic fiber

    CN110735202A

  • Intelligent combined processing system suitable for yak hair felt making

    CN113322585A

  • Yak hair core material for mattress and preparation method of yak hair core material

    CN113427846A