Diamond sintered body and tool having the same

By controlling the content, average particle size, and dislocation density of diamond particles, and combining them with an appropriate binding phase composition, a specific high-pressure and high-temperature sintering process is used to prepare a diamond sintered body with excellent resistance to chipping and wear. This solves the problems of insufficient tip chipping and wear resistance of diamond sintered bodies in cutting tools in the prior art, and achieves stability and wear resistance in efficient cutting processes.

CN116348624BActive Publication Date: 2024-11-19SUMITOMO ELECTRIC HARDMETAL CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202180071522.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-10-22
Filing Date
2021-10-05
Publication Date
2024-11-19
Estimated Expiration
2041-10-05

AI Technical Summary

Technical Problem

Existing diamond sintered materials are prone to tool tip damage in cutting tools and lack sufficient wear resistance in high-efficiency cutting processes.

Method used

By controlling the content, average particle size, and dislocation density of diamond particles, combined with an appropriate binding phase composition, and employing a specific high-pressure and high-temperature sintering process, diamond sintered bodies with excellent resistance to chipping and wear can be prepared.

Benefits of technology

It improves the chip resistance and wear resistance of diamond sintered bodies, making them suitable for machining various materials, especially exhibiting excellent cutting stability and wear resistance in high-efficiency cutting processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004186351030000081
    Figure BDA0004186351030000081
  • Figure BDA0004186351030000141
    Figure BDA0004186351030000141
  • Figure BDA0004186351030000151
    Figure BDA0004186351030000151
Patent Text Reader

Abstract

A diamond sintered body comprising diamond particles, wherein the content of the diamond particles is 80 volume % or more and 99 volume % or less relative to the diamond sintered body, the average particle size of the diamond particles is 0.1 μm or more and 50 μm or less, and the dislocation density of the diamond particles is 8.1×10 13 m ‑2 More than and less than 1.0×10 16 m ‑2 .
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to a diamond sintered body and a tool having a diamond sintered body. This application claims priority based on international application PCT / JP2020 / 039756 based on the Patent Cooperation Treaty (PCT) filed on October 22, 2020. All the contents recorded in the international application are incorporated by reference in this specification. Background Art

[0002] Diamond sintered bodies have excellent hardness and no hardness directionality or cleavage, so they are widely used in cutting tools, dressers, dies, and excavation drill bits.

[0003] Conventional diamond sintered bodies are obtained by sintering diamond powder as a raw material together with a sintering aid or a bonding material under conditions of high pressure and high temperature (generally, a pressure of about 5 to 8 GPa and a temperature of about 1300 to 2200°C) where diamond is thermodynamically stable. As sintering aids, iron group metals such as Fe, Co and Ni, carbonates such as CaCO3, etc. are used. As bonding materials, ceramics such as SiC, etc. are used.

[0004] For example, Japanese Patent Application Laid-Open No. 2005-239472 (Patent Document 1) discloses a high-strength and high-wear-resistant diamond sintered body comprising sintered diamond particles having an average particle size of 2 μm or less and a balance of a binder phase, wherein the content of the sintered diamond particles in the diamond sintered body is 80% by volume or more and 98% by volume or less, the binder phase contains at least one element selected from the group consisting of titanium, zirconium, hafnium, vanadium, niobium, tantalum, chromium and molybdenum having a content of 0.5% by mass or more and less than 50% by mass in the binder phase, and cobalt having a content of 50% by mass or more and less than 99.5% by mass in the binder phase, a part or all of the at least one element selected from the group consisting of titanium, zirconium, hafnium, vanadium, niobium, tantalum, chromium and molybdenum being present as carbide particles having an average particle size of 0.8 μm or less, the structure of the carbide particles being discontinuous, and adjacent diamond particles being bonded to each other.

[0005] In addition, Patent Document 1 discloses a method for manufacturing a high-strength and high-wear-resistant diamond sintered body, which is a method for manufacturing the high-strength and high-wear-resistant diamond sintered body, characterized in that sintering is carried out using a belt-type ultra-high pressure device under conditions of a pressure of greater than 5.7 GPa and less than 7.5 GPa and a temperature of greater than 1400°C and less than 1900°C.

[0006] Prior art literature

[0007] Patent Literature

[0008] Patent Document 1: Japanese Patent Application Publication No. 2005-239472 Summary of the invention

[0009] The diamond sintered body of the present disclosure comprises diamond particles, wherein:

[0010] The content of the diamond particles is 80% by volume or more and 99% by volume or less relative to the diamond sintered body.

[0011] The average particle size of the diamond particles is 0.1 μm or more and 50 μm or less.

[0012] The dislocation density of the diamond particles is 8.1×10 13 m -2 More than and less than 1.0×10 16 m -2 .

[0013] The tool disclosed in the present invention includes the above-mentioned diamond sintered compact. DETAILED DESCRIPTION

[0014] [Problems to be Solved by the Present Disclosure]

[0015] When the diamond sintered body of Patent Document 1 is used in cutting tools, the blade tip may be damaged. In addition, in recent years, more efficient cutting (e.g., high feed rate) is required, and the performance of the diamond sintered body is expected to be further improved (e.g., to suppress the wear caused by cutting, etc.).

[0016] The present disclosure has been made in view of the above circumstances, and an object of the present disclosure is to provide a diamond sintered body having excellent defect resistance and excellent wear resistance, and a tool including the diamond sintered body.

[0017] [Effects of the present disclosure]

[0018] According to the present disclosure, it is possible to provide a diamond sintered body having excellent defect resistance and excellent wear resistance, and a tool including the diamond sintered body.

[0019] [Description of Embodiments of the Present Disclosure]

[0020] First, embodiments of the present disclosure will be described by way of examples.

[0021] [1] A diamond sintered body according to one embodiment of the present disclosure includes diamond particles, wherein:

[0022] The content of the diamond particles is 80% by volume or more and 99% by volume or less relative to the diamond sintered body.

[0023] The average particle size of the diamond particles is 0.1 μm or more and 50 μm or less.

[0024] The dislocation density of the diamond particles is 8.1×10 13 m -2 More than and less than 1.0×10 16 m -2 .

[0025] The diamond sintered body has excellent defect resistance and excellent wear resistance. Here, "defect resistance" refers to the resistance to tool defect during material processing. "Wear resistance" refers to the resistance to tool wear during material processing.

[0026] [2] Preferably, the dislocation density of the diamond particles is 1.0×10 15 m -2 Above and 7.0×10 15 m -2 By defining in this way, a diamond sintered body having more excellent defect resistance and wear resistance is obtained.

[0027] [3] Preferably, the diamond sintered body further comprises a binder phase,

[0028] The above-mentioned bonding phase includes at least one selected from the group consisting of elemental metals, alloys and intermetallic compounds, wherein the elemental metals, alloys and intermetallic compounds include at least one metal element selected from the group consisting of Group IV elements, Group V elements, Group VI elements, iron, aluminum, silicon, cobalt and nickel of the periodic table, or,

[0029] The bonding phase includes at least one selected from the group consisting of compounds and solid solutions derived from the compounds, wherein the compounds and solid solutions derived from the compounds are composed of at least one metal element selected from the group consisting of Group IV elements, Group V elements, Group VI elements, iron, aluminum, silicon, cobalt and nickel of the periodic table and at least one non-metal element selected from the group consisting of nitrogen, carbon, boron and oxygen. By defining in this way, a diamond sintered body with better defect resistance is obtained.

[0030] [4] Preferably, the binder phase contains cobalt. By specifying this, a diamond sintered body having even better defect resistance is obtained.

[0031] [5] A tool according to one aspect of the present disclosure includes the above-mentioned diamond sintered compact.

[0032] Since the tool includes the diamond sintered body, it has excellent chipping resistance and excellent wear resistance in processing various materials.

[0033] [Details of the embodiments of the present disclosure]

[0034] The following is a detailed description of the embodiments of the present disclosure. In addition, the present disclosure is not limited to these examples. Here, in this specification, the expression in the form of "A to Z" refers to the upper and lower limits of the range (i.e., above A and below Z). When there is no record of units in A and only units in Z, the units of A are the same as the units of Z.

[0035] 《Diamond Sintered Body》

[0036] The diamond sintered body according to the present embodiment includes diamond particles, wherein:

[0037] The content of the diamond particles is 80% by volume or more and 99% by volume or less relative to the diamond sintered body.

[0038] The average particle size of the diamond particles is 0.1 μm or more and 50 μm or less.

[0039] The dislocation density of the diamond particles is 8.1×10 13 m -2 More than and less than 1.0×10 16 m -2 .

[0040] The diamond sintered body comprises diamond particles. That is, the diamond sintered body is basically composed of diamond particles. In one aspect of the present embodiment, the diamond particles can also be understood as diamond grains. The diamond sintered body preferably also comprises a bonding phase (binder) formed by one or both of a sintering aid and a bonding material. The diamond particles and the bonding phase will be described later.

[0041] The diamond sintered body is a polycrystal composed of a plurality of diamond particles. Therefore, the diamond sintered body does not have the directionality (anisotropy) and cleavage property of a single crystal, but has isotropic hardness and toughness in all directions.

[0042] The diamond sintered body may contain inevitable impurities within a range that exhibits the effects of the present embodiment. Examples of the inevitable impurities include hydrogen and oxygen.

[0043] <Diamond particles>

[0044] (Content ratio of diamond particles)

[0045] In the present embodiment, the content of the diamond particles is 80% by volume or more and 99% by volume or less, and preferably 80% by volume or more and 90% by volume or less, relative to the diamond sintered body.

[0046] The content (volume %) of diamond particles in the diamond sintered body and the content (volume %) of the binder phase described later can be confirmed by using an energy dispersive X-ray analyzer (EDX) (Octane Elect EDS system) (hereinafter also referred to as "SEM-EDX") attached with a scanning electron microscope (SEM) ("JSM-7800F" (trade name) manufactured by JEOL Ltd.) to observe the structure of the diamond sintered body, perform elemental analysis, etc. The specific measurement method is as follows.

[0047] First, cut off any position of the diamond sintered body to make a sample of a cross section containing the diamond sintered body. In the production of the cross section, a focused ion beam device, a cross-section polishing machine device, etc. can be used. Then, the above-mentioned cross section is observed using SEM to obtain a reflected electron image. In the reflected electron image, the area where the diamond particles are present is a black area, and the area where the binding phase is present is a gray area or a white area. The magnification when the above-mentioned cross section is observed using SEM is appropriately adjusted to the number of diamond particles observed in the measurement field of view to be more than 100. For example, when the average particle size of the diamond particles is 0.5 μm, the magnification when the above-mentioned cross section is observed using SEM can be 10,000 times. When the average particle size of the diamond particles is 30 μm, the magnification when the above-mentioned cross section is observed using SEM can be 200 times.

[0048] Next, the reflected electron image is binarized using image analysis software ("Win ROOF ver.7.4.5", "WinROOF2018", etc. of Mitani Shoji (strain). The image analysis software automatically sets an appropriate binarization threshold value based on the image information (the measurer does not set the threshold value at will). In addition, the inventor has confirmed that the measurement result does not change significantly even when the brightness of the image is changed, etc. According to the image after the binarization process, the area ratio of the pixels (pixels derived from diamond particles) from the dark field of view in the area of ​​the measurement field of view is calculated. By considering the calculated area ratio as volume %, the content (volume %) of the diamond particles can be obtained.

[0049] The content rate (volume %) of the binder phase can be determined by calculating the area ratio of pixels derived from the bright field (pixels derived from the binder phase) in the area of ​​the measurement field from the binarized image.

[0050] The inventors of the present invention have confirmed that, as long as the content (volume %) of diamond particles in the diamond sintered body and the content (volume %) of the binder phase described later are measured in the same sample, even if the selected position of the measurement field is changed and multiple calculations are performed, there is almost no deviation in the measurement results. In other words, the inventors of the present invention believe that even if the measurement field is arbitrarily set, the results will not change arbitrarily.

[0051] Furthermore, it can be confirmed that the pixels originating from the dark field are derived from the diamond particles by performing elemental analysis of the diamond sintered body using SEM-EDX.

[0052] (Average particle size of diamond particles)

[0053] The average particle size of the diamond particles is more than 0.1 μm and less than 50 μm, preferably more than 0.2 μm and less than 40 μm. By making the average particle size of the diamond particles more than 0.1 μm, the diamond particles are densely sintered to form a diamond sintered body with excellent defect resistance. By making the average particle size of the diamond particles less than 50 μm, a diamond sintered body with excellent cutting stability is formed when there is no anisotropy and the tip of the cutting tool is used as a cutting tool.

[0054] In the present embodiment, the average particle size of diamond particles refers to a value obtained by measuring the median particle sizes d50 of a plurality of diamond particles in each of the measurement fields of five arbitrarily selected locations and calculating the average value thereof.

[0055] First, cut off any position of the diamond sintered body to make a sample of a cross section containing the diamond sintered body. In the production of the cross section, a focused ion beam device, a cross-section polishing machine device, etc. can be used. Then, the above-mentioned cross section is observed using SEM to obtain a reflected electron image. In the reflected electron image, the area where the diamond particles are present is a black area, and the area where the binding phase is present is a gray area or a white area. The magnification when the above-mentioned cross section is observed using SEM is appropriately adjusted to the number of diamond particles observed in the measurement field of view to be more than 100. For example, when the average particle size of the diamond particles is 0.5 μm, the magnification when the above-mentioned cross section is observed using SEM can be 10,000 times. When the average particle size of the diamond particles is 30 μm, the magnification when the above-mentioned cross section is observed using SEM can be 200 times.

[0056] For each of the five SEM images, the equivalent circle diameter of each diamond particle was calculated using image processing software ("Win ROOF ver.7.4.5", "WinROOF2018", etc., of Mitani Shoji (strain)) under the state of separation of the grain boundaries of the diamond particles observed in the measurement field of view. At this time, the diamond particles that partially appear outside the above-mentioned measurement field of view are not counted.

[0057] Based on the calculated distribution of the equivalent circle diameters of the diamond particles, the median particle size d50 in each measurement field is calculated, and the average value thereof is calculated. This average value corresponds to the average particle size of the diamond particles.

[0058] Furthermore, the inventors of the present invention have confirmed that, as long as the average particle size of diamond particles is calculated in the same sample, even if the selected position of the measurement field of view in the diamond sintered body is changed and the calculation is performed multiple times, there is almost no deviation in the measurement result. In other words, the inventors of the present invention believe that even if the measurement field of view is arbitrarily set, the result will not change arbitrarily.

[0059] (Dislocation density of diamond particles)

[0060] The dislocation density of the diamond particles is 8.1×10 13 m -2 More than and less than 1.0×10 16 m -2 , preferably 1.0×10 15 m -2 Above and 7.0×10 15 m -2 By making the dislocation density of diamond particles less than 1.0×10 16 m -2 , thereby forming a diamond sintered body that suppresses the occurrence of cracks in diamond particles and has excellent defect resistance. In addition, the thermal conductivity of the diamond sintered body is high. Therefore, thermal wear caused by the temperature increase of the blade tip during cutting can be suppressed. In addition, the inventors of the present invention have confirmed that it is impossible to produce diamond particles with a dislocation density of less than 8.1×10 13 m -2 of diamond sintered body.

[0061] In the past, no attention has been paid to the correlation between the dislocation density of diamond particles in a diamond sintered body and the physical properties of the diamond sintered body. Therefore, the inventors of the present invention have conducted in-depth research on the relationship between the dislocation density of diamond particles in a diamond sintered body and the defect resistance and wear resistance of the diamond sintered body. As a result, it was found for the first time that if the dislocation density of diamond particles is reduced compared with the existing diamond sintered bodies, the generation of cracks caused by the slip movement of dislocations in the diamond particles can be suppressed, thereby improving the defect resistance. In addition, it was found for the first time that if the dislocation density of diamond particles is reduced, the wear during cutting can be suppressed. It is believed that the reason is that by reducing the dislocation density, the heat generated during cutting can be effectively transferred to the entire diamond sintered body, and the wear of the diamond sintered body caused by heat can be suppressed. In addition, it can be seen from this investigation that the dislocation density of diamond particles in the previous diamond sintered body (for example, the diamond sintered body described in Patent Document 1) is 1.01×10 16 m -2 Above and less than 1.18×10 16 m -2 .

[0062] In this specification, the dislocation density of a diamond sintered body is measured at a large-scale radiation light facility (for example, Kyushu Synchrotron Light Research Center (Saga Prefecture)). Specifically, the dislocation density is measured by the following method.

[0063] A test body consisting of a diamond sintered body was prepared. The size of the test body was 3 mm × 6 mm on the observation surface and 0.4 mm in thickness. The observation surface of the test body was mirror-polished using a diamond polishing liquid with an average particle size of 3 μm, and then immersed in hydrochloric acid for 72 hours. As a result, in the observation surface of the test body, the binding phase was dissolved in the hydrochloric acid, and the diamond particles remained.

[0064] The test body was subjected to X-ray diffraction measurement under the following conditions to obtain line profiles of diffraction peaks from various planes, which are the main orientations of diamond: (111), (220), (311), (331), (422), (440), and (531).

[0065] (X-ray diffraction measurement conditions)

[0066] X-ray source: radiation

[0067] Device conditions: Detector NaI (fluorescence cutoff by appropriate ROI).

[0068] Energy: 18keV (wavelength: )

[0069] Spectroscopic crystal: Si(111)

[0070] Entrance slit: width 3mm × height 0.5mm

[0071] Light receiving slit: double slit (width 3mm × height 0.5mm)

[0072] Reflector: Platinum coated mirror

[0073] Incident angle: 2.5mrad

[0074] Scanning method: 2θ-θscan

[0075] Peaks to be measured: Seven peaks of diamond: (111), (220), (311), (331), (422), (440), and (531). However, when it is difficult to obtain the outline due to texture, orientation, etc., the peak of the surface index is excluded.

[0076] Measurement conditions: The measurement points are set to nine or more points in the full width at half maximum corresponding to each measurement peak. The peak top intensity is 2000 counts or more. Since the edge of the peak is also used for analysis, the measurement range is about 10 times the full width at half maximum.

[0077] The line profile obtained by the above-mentioned X-ray diffraction measurement is formed into a shape that includes both the real extension caused by physical quantities such as the inhomogeneous strain of the test body and the extension caused by the device. In order to obtain the inhomogeneous strain and the crystallite size, the components caused by the device are removed from the measured line profile to obtain the real line profile. The real line profile is obtained by fitting the obtained line profile and the line profile caused by the device using a pseudo-Voigt function, and subtracting the line profile caused by the device. As a standard sample for removing the diffraction line expansion caused by the device, LaB6 is used. In addition, when using radiated light with high parallelism, the diffraction line expansion caused by the device can also be regarded as 0.

[0078] The obtained true line profile is analyzed using the modified Williamson-Hall method and the modified Warren-Averbach method to calculate the dislocation density. The modified Williamson-Hall method and the modified Warren-Averbach method are known line profile analysis methods for obtaining the dislocation density.

[0079] The modified Williamson-Hall method is represented by the following formula (I).

[0080] [Number 1]

[0081]

[0082] In the above formula (I), ΔK represents the half-value width of the line profile. D represents the crystallite size. M represents the configuration parameter. b represents the Burgers vector. ρ represents the dislocation density. K represents the scattering vector. O(K 2 C) represents K 2 The higher order terms of C. C represents the average value of the contrast factor.

[0083] C in the above formula (I) is represented by the following formula (II).

[0084] C=C h00 [1-q(h 2 k 2 +h 2 l 2 +k 2 l 2 ) / (h 2 +k 2 +l 2 ) 2 ] (II)

[0085] In the above formula (II), the contrast factors C of screw dislocation and edge dislocation are h00 The coefficient q related to the contrast factor is calculated using the code ANIZC, with the slip system as <110> {111}, elastic stiffness C 11 1076GPa, C 12 125GPa, C 44 In the above formula (II), h, k and l correspond to the Miller index (hkl) of diamond respectively. h00 The ratio of screw dislocations is 0.183 and that of edge dislocations is 0.204. The coefficient q related to the contrast factor is 1.35 for screw dislocations and 0.30 for edge dislocations. In addition, the ratio of screw dislocations is fixed at 0.5 and that of edge dislocations is fixed at 0.5.

[0086] In addition, the contrast factor C is used between dislocation and inhomogeneous strain to establish the relationship of the following formula (III). In the following formula (III), R e represents the effective radius of dislocation. ε(L) represents the inhomogeneous strain.

[0087] <ε(L) 2 >=(ρCb 2 / 4π)ln(R e / L) (III)

[0088] Based on the relationship of the above formula (III) and the Warren-Averbach formula, it can be expressed as the following formula (IV), and as a modified Warren-Averbach method, the dislocation density ρ and the crystallite size can be obtained. In the following formula (IV), A(L) represents the Fourier series. A S (L) represents the Fourier series related to the crystallite size. L represents the Fourier length.

[0089] lnA(L)=lnA S (L)-(πL 2 ρb 2 / 2)ln(R e / L)(K 2 C)+O(K 2 C) 2 (IV)

[0090] The details of the modified Williamson-Hall method and the modified Warren-Averbach method are described in “T. Ungar and A. Borbely, “The effect of dislocation contrast on x-ray linebroadening: A new approach to line profile analysis” Appl. Phys. Lett., vol. 69, no. 21, p. 3173, 1996.” and “T. Ungar, S. Ott, P. Sanders, A. Borbely, J. Weertman, “Dislocations, grain size and planar faults in nanostructured copper determined by high resolution X-ray diffraction and a new procedure of peakprofile analysis” Acta Mater., vol. 46, no. 10, pp. 3693-3699, 1998.”.

[0091] The inventors of the present invention have confirmed that as long as the dislocation density of diamond particles is measured in the same sample, there is almost no deviation in the measurement results even if the selected position of the measurement range is changed and multiple calculations are performed. In other words, the inventors of the present invention believe that even if the measurement field of view is arbitrarily set, the results will not change arbitrarily.

[0092] <Combination Phase>

[0093] In this embodiment, preferably, the diamond sintered body further comprises a binding phase.

[0094] The above-mentioned bonding phase includes at least one selected from the group consisting of a single metal, an alloy and an intermetallic compound, wherein the single metal, the alloy and the intermetallic compound include at least one metal element selected from the group consisting of Group IV elements, Group V elements, Group VI elements, iron, aluminum, silicon, cobalt and nickel of the periodic table (hereinafter also referred to as "Group A"), or,

[0095] The above-mentioned binding phase includes at least one selected from the group consisting of compounds and solid solutions derived from the above-mentioned compounds, wherein the compounds and solid solutions derived from the above-mentioned compounds are composed of at least one metal element selected from the group consisting of Group IV elements, Group V elements, Group VI elements, iron, aluminum, silicon, cobalt and nickel (Group A) of the periodic table and at least one non-metal element selected from the group consisting of nitrogen, carbon, boron and oxygen (hereinafter also referred to as "Group B"). In other words, the above-mentioned binding phase can be any one of the following forms (a) to (f).

[0096] (a) The bonding phase is composed of at least one selected from the group consisting of a single metal, an alloy, and an intermetallic compound, wherein the single metal, the alloy, and the intermetallic compound contain at least one metal element selected from Group A.

[0097] (b) The bonding phase includes at least one selected from the group consisting of a single metal, an alloy, and an intermetallic compound, wherein the single metal, the alloy, and the intermetallic compound include at least one metal element selected from Group A.

[0098] (c) The above-mentioned binding phase is composed of at least one selected from the group consisting of compounds and solid solutions derived from the above-mentioned compounds, and the compounds and solid solutions derived from the above-mentioned compounds are composed of at least one metal element selected from group A and at least one non-metal element selected from group B.

[0099] (d) The above-mentioned binding phase contains at least one selected from the group consisting of compounds and solid solutions derived from the above-mentioned compounds, and the compounds and solid solutions derived from the above-mentioned compounds are composed of at least one metal element selected from group A and at least one non-metal element selected from group B.

[0100] (e) The above-mentioned bonding phase is composed of at least one selected from the group consisting of elemental metals, alloys and intermetallic compounds, and at least one selected from the group consisting of compounds and solid solutions derived from the above-mentioned compounds, wherein the elemental metals, alloys and intermetallic compounds contain at least one metal element selected from group A, and the compounds and solid solutions derived from the above-mentioned compounds are composed of at least one metal element selected from group A and at least one non-metallic element selected from group B.

[0101] (f) The above-mentioned bonding phase includes at least one selected from the group consisting of elemental metals, alloys and intermetallic compounds, and at least one selected from the group consisting of compounds and solid solutions derived from the above-mentioned compounds, wherein the elemental metals, alloys and intermetallic compounds contain at least one metal element selected from group A, and the compounds and solid solutions derived from the above-mentioned compounds are composed of at least one metal element selected from group A and at least one non-metallic element selected from group B.

[0102] The fourth group elements of the periodic table include titanium (Ti), zirconium (Zr) and hafnium (Hf), the fifth group elements include vanadium (V), niobium (Nb) and tantalum (Ta), and the sixth group elements include chromium (Cr), molybdenum (Mo) and tungsten (W).

[0103] In one aspect of this embodiment, the bonding phase preferably includes at least one selected from the group consisting of cobalt, titanium, iron, tungsten and boron, and more preferably includes cobalt.

[0104] The composition of the binder phase contained in the diamond sintered body can be determined by EDX with SEM as described above.

[0105] (Content ratio of the binding phase)

[0106] The content of the bonding phase is preferably 1% by volume or more and 20% by volume or less, more preferably 10% by volume or more and 20% by volume or less relative to the diamond sintered body. The content (volume %) of the bonding phase can be confirmed by using EDX with SEM to observe the structure of the diamond sintered body, perform elemental analysis, etc.

[0107] "tool"

[0108] The diamond sintered body of the present embodiment has excellent defect resistance and wear resistance, and can therefore be suitably used in cutting tools, wear-resistant tools, grinding tools, friction stir welding tools, etc. That is, the tool of the present embodiment has the above-mentioned diamond sintered body. The above-mentioned tool has excellent defect resistance and excellent wear resistance in the processing of various materials. When the above-mentioned tool is a cutting tool, the above-mentioned cutting tool is particularly suitable for rotary cutting and turning of aluminum alloys (for example, A390, AC4C) and the like.

[0109] The above-mentioned tool may be composed of a diamond sintered body in its entirety, or only a portion thereof (for example, a cutting edge portion in the case of a cutting tool) may be composed of a diamond sintered body.

[0110] Examples of the cutting tool include drills, end mills, indexable cutting inserts for drills, indexable cutting inserts for end mills, indexable cutting inserts for milling, indexable cutting inserts for turning, metalworking saws, gear cutting tools, reamers, taps, cutting tools, and the like.

[0111] Examples of the wear-resistant tool include a punch, a scriber, a scribing wheel, a dresser, and the like.

[0112] Examples of the grinding tool include grinding stones and the like.

[0113] 《Method for producing diamond sintered body》

[0114] The method for producing a diamond sintered body according to the present embodiment comprises:

[0115] A step of preparing raw material powder of diamond particles and raw material powder of a binding phase;

[0116] A step of mixing the raw material powder of the diamond particles and the raw material powder of the binder phase to obtain a mixed powder;

[0117] A step of sintering the mixed powder at a sintering pressure of 4 GPa to less than 5 GPa, at a sintering temperature of 1400° C. to 1550° C., and for a sintering time of 15 minutes to 60 minutes; and

[0118] The mixed powder is heated at a holding temperature of 1600° C. to 1900° C. for a holding time of 50 minutes to 190 minutes under a holding pressure of 6.5 GPa to 8 GPa to reduce dislocations in the diamond particles.

[0119] <Step of Preparing Raw Material Powder of Diamond Particles and Raw Material Powder of Binder Phase>

[0120] In this step, raw material powder of diamond particles (hereinafter also referred to as "diamond powder") and raw material powder of a binder phase (hereinafter also referred to as "binding phase raw material powder") are prepared. The diamond powder is not particularly limited, and known diamond particles can be used as the raw material powder.

[0121] The average particle size of the diamond powder is not particularly limited, and can be, for example, 0.1 μm or more and 50 μm or less.

[0122] The binder phase raw material powder is not particularly limited as long as it is a powder containing elements constituting the binder phase. Examples of the binder phase raw material powder include cobalt powder, titanium powder, etc. The binder phase raw material powder may be used alone or in combination of multiple powders, depending on the composition of the target binder phase.

[0123] <Step of Obtaining Mixed Powder>

[0124] In this step, the raw material powder of the diamond particles (diamond powder) and the raw material powder of the bonding phase (bonding phase raw material powder) are mixed to obtain a mixed powder. At this time, the diamond powder and the bonding phase raw material powder can be mixed in any proportion so that the content of the diamond particles in the diamond sintered body is within the above range.

[0125] The method for mixing the two powders is not particularly limited, and may be a mixing method using an attritor or a mixing method using a ball mill. The mixing method may be a wet method or a dry method.

[0126] <Step of sintering the mixed powder>

[0127] In this step, the mixed powder is sintered at a sintering pressure of 4 GPa to less than 5 GPa, at a sintering temperature of 1400° C. to 1550° C., and for a sintering time of 15 minutes to 60 minutes.

[0128] In the present embodiment, the path from the state of room temperature (23±5° C.) and atmospheric pressure to the state of the above-mentioned sintering pressure and sintering temperature is not particularly limited.

[0129] The high pressure and high temperature generator used in the method for producing a diamond sintered body of the present embodiment is not particularly limited as long as it is a device that can obtain the target pressure and temperature conditions. From the viewpoint of improving productivity and workability, the high pressure and high temperature generator is preferably a belt-type high pressure and high temperature generator. In addition, the container for storing the mixed powder is not particularly limited as long as it is made of a material that is resistant to high pressure and high temperature, for example, tantalum (Ta), niobium (Nb), etc. are preferably used.

[0130] In order to prevent impurities from being mixed into the diamond sintered body, for example, the mixed powder is first placed in a capsule made of a high melting point metal such as Ta, Nb, etc., and heated and sealed in a vacuum to remove adsorbed gas and air from the mixed powder. Afterwards, the above-mentioned process of sintering the mixed powder and the process of reducing dislocations in the diamond particles described later are preferably performed. In one aspect of the present embodiment, after the above-mentioned process of sintering the mixed powder, the mixed powder is preferably not taken out from the capsule made of the high melting point metal, and the process of reducing dislocations in the diamond particles is continued in an unchanged state.

[0131] The sintering pressure is preferably 4 GPa or more and less than 5 GPa, and more preferably 4.5 GPa or more and less than 5 GPa.

[0132] The sintering temperature is preferably 1400°C or higher and 1550°C or lower, and more preferably 1450°C or higher and 1550°C or lower.

[0133] The sintering time is preferably 15 minutes to 60 minutes, more preferably 15 minutes to 20 minutes.

[0134] <Step of Reducing Dislocations in Diamond Particles>

[0135] In this process, the mixed powder is heated at a holding pressure of 6.5 GPa to 8 GPa, a holding temperature of 1600°C to 1900°C, and a holding time of 50 minutes to 190 minutes to reduce dislocations in the diamond particles. Thus, the diamond sintered body disclosed in the present invention is obtained. The inventors of the present invention believe that this process promotes the dissolution and re-precipitation reaction of diamond, but the re-precipitated diamond particles have fewer dislocations, so a diamond sintered body with fewer dislocations is obtained.

[0136] The holding pressure is preferably 6.5 GPa or more and 8 GPa or less, and more preferably 6.5 GPa or more and 7 GPa or less.

[0137] The holding temperature is preferably 1600°C or higher and 1900°C or lower, and more preferably 1600°C or higher and 1700°C or lower.

[0138] The retention time is preferably 50 minutes to 190 minutes, more preferably 60 minutes to 180 minutes.

[0139] Example

[0140] The present embodiment will be described in more detail by way of examples, but the present embodiment is not limited to these examples.

[0141] 《Production of Diamond Sintered Body》

[0142] <Step of Preparing Raw Material Powder of Diamond Particles and Raw Material Powder of Binder Phase>

[0143] As raw material powders, powders having average particle sizes or compositions shown in Table 1-1 and Table 1-2 were prepared.

[0144] Table 1-1

[0145]

[0146] Table 1-2

[0147]

[0148] <Step of Obtaining Mixed Powder>

[0149] In order to obtain a diamond sintered body having the composition described in Table 3-1 or Table 3-2, the prepared raw material powders are added in various proportions, and mixed in a dry manner using a ball mill to produce a mixed powder. Here, as described later, the mixed powder is sintered in contact with a disk made of WC-6%Co cemented carbide. Therefore, it is believed that during sintering, cobalt and tungsten are melt-infiltrated from the disk into the diamond sintered body, increasing the cobalt content and the tungsten content in the diamond sintered body. The proportion of each raw material powder is determined by considering the increase in the cobalt content and the increase in the tungsten content in advance.

[0150] <Step of sintering the mixed powder>

[0151] Next, the mixed powder was placed in a Ta capsule in contact with a WC-6%Co cemented carbide disk, and heated and sealed in a vacuum. Thereafter, the mixed powder was sintered using a high pressure and high temperature generator at the sintering pressure, sintering temperature, and sintering time shown in Table 2-1 or Table 2-2.

[0152] <Step of Reducing Dislocations in Diamond Particles>

[0153] After the step of sintering the mixed powder, the mixed powder was heated at the holding pressure, holding temperature and holding time shown in Table 2-1 or Table 2-2. This step was not performed for Sample 8 and Sample 28. Diamond sintered bodies of Samples 1 to 32 were manufactured through the above steps.

[0154] Table 2-1

[0155]

[0156] Table 2-2

[0157]

[0158] 《Evaluation of properties of diamond sintered compact》

[0159] <Composition of Diamond Sintered Body>

[0160] The content ratio (volume ratio) of diamond particles and binding phase in the diamond sintered body was measured. The specific measurement method is the same as the method described in the above-mentioned [Details of the Embodiments of the Present Disclosure] column, so the description thereof will not be repeated. It was confirmed that the content ratio of diamond particles in the diamond sintered body in each sample was as shown in Table 3-1 and Table 3-2 (refer to the "Content Ratio" column).

[0161] <Average particle size of diamond particles>

[0162] The average particle size of the diamond particles in the diamond sintered body was measured. The specific measurement method is the same as the method described in the above-mentioned [Details of the Embodiments of the Present Disclosure] column, so the description thereof will not be repeated. The results are shown in Table 3-1 and Table 3-2 (refer to the "Average Particle Size" column).

[0163] <Composition of Binding Phase>

[0164] The composition of the binder phase in the diamond sintered body was determined by SEM-EDX. The specific determination method is the same as the method described in the above-mentioned [Details of the Embodiments of the Present Disclosure] column, so the description thereof will not be repeated. The results are shown in Table 3-1 and Table 3-2 (refer to the "Composition of the binder phase" column).

[0165] <Dislocation Density of Diamond Particles>

[0166] The dislocation density of the diamond particles in the diamond sintered body was measured. The specific measurement method is the same as the method described in the above-mentioned [Details of the Embodiments of the Present Disclosure] column, so the description thereof will not be repeated. The results are shown in Table 3-1 and Table 3-2 (refer to the "Dislocation Density" column).

[0167] 《Evaluation of tools with diamond sintered body》

[0168] <Cutting test 1: Turning test>

[0169] Cutting tools (holder: CSRP R3225-N12, blade: SPGN120304, a tool having the above-mentioned diamond sintered body at the tip of the blade) were made using the diamond sintered bodies of samples 1 to 14 made as described above, and a turning test was carried out. The cutting conditions of the turning test are as follows. In the above-mentioned turning test, the longer the cutting distance (km), the more it can be evaluated as a cutting tool with excellent defect resistance and wear resistance. The results are shown in Table 3-1. In cutting test 1, samples 1 to 7, sample 10, and samples 12 to 14 correspond to embodiments. Samples 8, sample 9, and sample 11 correspond to comparative examples.

[0170] (Cutting conditions for turning test)

[0171] Cutting material: A390 (φ120mm×280mm)

[0172] Cutting speed: 800m / min

[0173] Feed rate: 0.12mm / rev

[0174] Cutting: 0.5mm

[0175] Coolant: wet

[0176] Evaluation method: The outer diameter of the workpiece is turned, and the cutting distance (km) until the average flank wear width of the cutting tool reaches 250μm is measured.

[0177] <Cutting test 2: Turning test>

[0178] The diamond sintered bodies of samples 15 to 20 prepared as described above were used to make cutting tools (holder: CSRP R3225-N12, insert: SPGN120308, a tool having the diamond sintered body at the tip of the insert), and a turning test was performed. The cutting conditions of the turning test are as follows. In the turning test, the longer the cutting distance (km), the more it can be evaluated as a cutting tool with excellent defect resistance and wear resistance.

[0179] The results are shown in Table 3-1. In the cutting test 2, samples 15 to 19 correspond to Examples, and sample 20 corresponds to Comparative Example.

[0180] (Cutting conditions for turning test)

[0181] Cutting material: Ti-6Al-4V

[0182] Cutting speed: 250m / min

[0183] Feed rate: 0.1mm / rev

[0184] Cutting: 0.4mm

[0185] Coolant: wet

[0186] Evaluation method: The outer diameter of the workpiece is turned, and the cutting distance (km) until the average flank wear width of the cutting tool reaches 200 μm is measured.

[0187] Table 3-1

[0188]

[0189] <Results>

[0190] According to the results of cutting test 1, the cutting tools of samples 1 to 7, 10, and 12 to 14 (cutting tools of the embodiment) obtained good results of cutting distance of more than 10.1 km. On the other hand, the cutting tools of samples 8, 9, and 11 (cutting tools of the comparative example) produced notches in the initial stage of cutting, and the cutting distance could not be obtained. From the above results, it can be seen that the cutting tools of the embodiment are superior in defect resistance and wear resistance compared with the cutting tools of the comparative example.

[0191] According to the results of cutting test 2, the cutting tools of samples 15 to 19 (cutting tools of the embodiment) obtained good results of cutting distance of more than 3.5 km. On the other hand, the cutting tool of sample 20 (cutting tool of the comparative example) had a chip in the initial stage of cutting, and the cutting distance could not be obtained. From the above results, it can be seen that the cutting tools of the embodiment are superior in defect resistance and wear resistance compared with the cutting tools of the comparative example.

[0192] <Cutting test 3: Turning test>

[0193] The diamond sintered bodies of samples 21 to 32 prepared as described above were used to prepare cutting tools (holder: CSRP R3225-N12, blade: SPGN120304, a tool having the above-mentioned diamond sintered body at the tip of the blade), and a turning test was performed. The cutting conditions of the turning test are as follows. In the above-mentioned turning test, the longer the cutting distance (km), the more it can be evaluated as a cutting tool with excellent defect resistance and wear resistance. The results are shown in Table 3-2. In cutting test 3, samples 21 to 27, sample 30 and sample 32 are equivalent to embodiments. Samples 28, sample 29 and sample 31 are equivalent to comparative examples.

[0194] (Cutting conditions for turning test)

[0195] Workpiece: AC4C (φ120mm×280mm)

[0196] Cutting speed: 1200m / min

[0197] Feed rate: 0.2mm / rev

[0198] Incision: 1.2mm

[0199] Coolant: wet

[0200] Evaluation method: The outer diameter of the material being cut is turned, and the cutting distance (km) until the average flank wear width of the cutting tool reaches 250μm is measured.

[0201] Table 3-2

[0202]

[0203] <Results>

[0204] According to the results of cutting test 3, the cutting tools of samples 21 to 27, 30 and 32 (cutting tools of the embodiment) obtained good results of cutting distance of more than 12.2 km. On the other hand, the cutting tools of samples 28, 29 and 31 (cutting tools of the comparative example) had notches in the initial stage of cutting, and the cutting distance could not be obtained. From the above results, it can be seen that the cutting tools of the embodiment are superior in defect resistance and wear resistance compared with the cutting tools of the comparative example.

[0205] As mentioned above, although the embodiment and the example of this disclosure were described, it is also planned from the beginning that the configurations of each embodiment and the example described above are appropriately combined or variously modified.

[0206] The embodiments and examples disclosed herein are illustrative in all aspects and should not be construed as restrictive. The scope of the present invention is indicated by the claims rather than the above description, and is intended to include all modifications within the meaning and scope equivalent to the claims.

Claims

1. A diamond sintered body comprising diamond particles and a binding phase, in, The bonding phase comprises tungsten and cobalt, The content of the diamond particles is 80% by volume or more and 99% by volume or less relative to the diamond sintered body, The average particle size of the diamond particles is greater than or equal to 0.1 μm and less than or equal to 50 μm. The dislocation density of the diamond particles is 8.1×10 13 m -2 More than and less than 1.0×10 16 m -2 .

2. The diamond sintered body according to claim 1, in, The dislocation density of the diamond particles is 1.0×10 15 m -2 Above and 7.0×10 15 m -2 the following.

3. The diamond sintered body according to claim 1 or 2, in, The bonding phase comprises at least one selected from the group consisting of elemental metals, alloys and intermetallic compounds, wherein the elemental metals, alloys and intermetallic compounds comprise at least one metal element selected from the group consisting of Group IV elements, Group V elements, Group VI elements, iron, aluminum, silicon and nickel of the periodic table, or, The binding phase comprises at least one selected from the group consisting of compounds and solid solutions derived from the compounds, wherein the compounds and solid solutions derived from the compounds are composed of at least one metal element selected from the group consisting of Group IV elements, Group V elements, Group VI elements, iron, aluminum, silicon and nickel of the periodic table and at least one non-metal element selected from the group consisting of nitrogen, carbon, boron and oxygen, The Group VI elements are Group VI elements other than tungsten.

4. A tool, in, The tool comprises the diamond sintered body according to any one of claims 1 to 3.