A method for solving the problem of nitrogen oxides generated during the nitric acid dissolution process of uranium trioxide product
By stirring and dissolving hydrogen peroxide and uranium octoxide products in a nitric acid solution during the uranium purification and conversion process, the problem of nitrogen oxide production during the dissolution process of nitric acid is solved, reducing the production of nitrogen oxides and acid consumption, and improving the Economic benefits.
Patent Information
- Application Number
- CN202111615783.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-12-27
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2041-12-27
AI Technical Summary
During the uranium purification and conversion process, a large amount of harmful nitrogen oxide gas is generated during the nitric acid dissolution of uranium octoxide products, resulting in increased environmental pressure and increased production costs.
By adding hydrogen peroxide and uranium octoxide products into the nitric acid solution in a specific ratio, stirring and dissolving to ensure that the nitric acid concentration is not less than 2.6 mol/L, and proceeding under appropriate heating and stirring conditions, the production of nitrogen oxides can be reduced.
It significantly reduces the production of nitrogen oxides, reduces equipment investment and wastewater production, and improves the economic benefits of the process.
Abstract
Description
Technical Field
[0001] The invention relates to the field of uranium purification and conversion, and in particular to a method for solving the problem of nitrogen oxides generated in the nitric acid dissolution process of uranium trioxide products. Background Art
[0002] Uranium trioxide (U3O8) is the main uranium concentrate product. During the nitric acid dissolution process of U3O8 in the uranium purification and conversion process, a large amount of nitrogen oxide harmful gas is produced, which is not conducive to the environmental protection and economy of the process.
[0003] The uranium in the U3O8 material contains both low-valent +4 uranium and high-valent +6 uranium. Its nitric acid dissolution process requires not only acidolysis but also oxidation. When nitric acid and the reducing substance +4 uranium undergo oxidation reaction, the reduced products will also differ depending on the concentration of nitric acid. Under normal circumstances, concentrated nitric acid will be reduced to nitrogen dioxide when reacting with reducing substances, and dilute nitric acid will be reduced to nitric oxide when reacting with reducing substances. Similarly, when U3O8 is dissolved with nitric acid, the following reaction occurs:
[0004] U3O8+8HNO3(concentrated)→3UO2(NO3)2+2NO2↑+4H2O
[0005] 3U3O8+20HNO3(dilute)→9UO2(NO3)2+2NO↑+10H2O
[0006] Nitrogen oxides are harmful to humans and the environment to varying degrees, and bring great environmental pressure to enterprises. They need to be collected and treated using capture devices, which increases production and operating costs. Summary of the invention
[0007] The technical problem to be solved by the present invention is to provide a method for solving the problem of nitrogen oxides generated during the nitric acid dissolution process of uranium trioxide products, thereby significantly reducing the amount of nitrogen oxides generated during the dissolution process, alleviating the pollution problem of nitrogen oxides, and improving the economic benefits of the process.
[0008] The present invention provides a method for solving the problem of nitrogen oxides generated during the nitric acid dissolution process of uranium trioxide product, comprising the following steps:
[0009] Add hydrogen peroxide and uranium trioxide product into nitric acid solution according to the proportion, and stir to dissolve;
[0010] The molar ratio of uranium trioxide product to hydrogen peroxide is less than or equal to 1;
[0011] The concentration of nitric acid shall not be less than 2.6 mol / L.
[0012] Preferably, it specifically includes:
[0013] Heat the nitric acid solution, then add hydrogen peroxide, mix well, and then add the uranium octoxide product.
[0014] Preferably, the heating temperature is no higher than 60°C.
[0015] Preferably, the stirring and dissolving time is not less than 15 minutes.
[0016] Preferably, the concentration of the nitric acid solution is 3-6 mol / L.
[0017] Preferably, the uranium content of the uranium trioxide product is 84.8%.
[0018] Compared with the prior art, the method of the present invention for solving the problem of nitrogen oxides generated during the nitric acid dissolution process of uranium trioxide product solves the problem of nitrogen oxides gas generated during the nitric acid dissolution process of U3O8, reduces equipment investment and the generation of absorption wastewater, reduces the acid consumption of nitric acid dissolution, and improves economic benefits. The technology is economical, simple and practical. DETAILED DESCRIPTION
[0019] In order to further understand the present invention, the embodiments of the present invention are described below in conjunction with examples, but it should be understood that these descriptions are only for further illustrating the features and advantages of the present invention, rather than limiting the present invention.
[0020] The embodiment of the present invention discloses a method for solving the problem of nitrogen oxides generated during the nitric acid dissolution process of uranium trioxide product, comprising the following steps:
[0021] Add hydrogen peroxide and uranium trioxide product into nitric acid solution according to the proportion, and stir to dissolve;
[0022] The molar ratio of uranium trioxide product to hydrogen peroxide is less than or equal to 1;
[0023] The concentration of nitric acid is not less than 2.6 mol / L, preferably 3 to 6 mol / L.
[0024] Preferably, it specifically includes:
[0025] Heat the nitric acid solution, then add hydrogen peroxide, mix well, and then add the uranium octoxide product.
[0026] The heating temperature is not higher than 60°C.
[0027] The stirring and dissolving time is not less than 15 minutes.
[0028] The uranium content of the uranium trioxide product is 84.8%.
[0029] The invention solves the problem that 1) nitrogen oxide gas is generated during the dissolution of U3O8 in nitric acid, reduces equipment investment and generates absorption wastewater.
[0030] The uranium in U3O8 material contains both low-valent +4 uranium and high-valent +6 uranium. Its nitric acid dissolution process requires not only acid hydrolysis but also oxidation. When nitric acid undergoes oxidation reaction with reducing substances, it will be reduced to nitrogen oxides such as nitrogen dioxide and nitric oxide. Nitrogen oxides need to be collected and treated with additional capture devices.
[0031] O2 in H2O2 reagent 2- It is a strong oxidant. The invention adds H2O2 reagent in a certain proportion to make the O2 2- The redox reaction with +4 uranium in U3O8 material produces the following reaction:
[0032] U3O8+H2O2+6HNO3→3UO2(NO3)2+4H2O
[0033] It avoids the reduction of nitric acid to nitrogen oxides, and can effectively solve the problem of nitrogen oxides produced by U3O8 during the dissolution of nitric acid, eliminating the investment in nitrogen oxide absorption equipment and reducing the generation of absorption wastewater.
[0034] 2) The acid consumption of nitric acid dissolution is reduced, and the economic benefits are improved.
[0035] The nitric acid dissolution process of U3O8 material requires not only acid hydrolysis but also oxidation. The invention adds H2O2 reagent in a certain proportion to make the O2 2- The nitric acid undergoes an oxidation-reduction reaction with the +4-valent uranium in the U3O8 material, thereby reducing the consumption of nitric acid for the oxidation reaction of the +4-valent uranium during the dissolution of the U3O8 material.
[0036] In order to further understand the present invention, the method for solving the problem of nitrogen oxides generated during the nitric acid dissolution process of uranium trioxide product provided by the present invention is described in detail below in conjunction with the embodiments. The protection scope of the present invention is not limited by the following embodiments.
[0037] Example 1
[0038] 100ml of a solution with a nitric acid concentration of 6mol / L is used, the uranium content is calculated at a concentration of 300g / L, the molar ratio of U3O8 to H2O2 products is 1:1, and the uranium content of the U3O8 product is 84.8%, that is, 35.4g of U3O8 product and 4.8g of H2O2 reagent with a content of 30% need to be added to 100mol of nitric acid solution. The nitric acid solution is heated to 60°C using a water bath thermostatic agitator. Subsequently, the H2O2 reagent is pre-added to the nitric acid solution, mixed evenly, and then the U3O8 product is added. The stirring and dissolving time is 15min. During the dissolution process, the gas is collected and analyzed. After dissolution, the solution is filtered and the insoluble slag is dried and weighed. The dissolution rate of the uranium product is calculated to be 98.01%. The amount of nitrogen oxides produced during the dissolution process is determined to be reduced by more than 99% compared with the method of dissolving the U3O8 product without adding the H2O2 reagent.
[0039] Example 2
[0040] 100ml of a solution with a nitric acid concentration of 6mol / L is used, the uranium content is calculated at a concentration of 300g / L, the molar ratio of U3O8 to H2O2 products is 1:1.1, and the uranium content of the U3O8 product is 84.8%, that is, 35.4g of U3O8 product and 5.2g of H2O2 reagent with a content of 30% are added to 100mol of nitric acid solution. The nitric acid solution is heated to 60°C using a water bath thermostatic agitator. Subsequently, the H2O2 reagent is pre-added to the nitric acid solution, mixed evenly, and then the U3O8 product is added. The stirring and dissolving time is 15min. During the dissolution process, the gas is collected and analyzed. After dissolution, the solution is filtered and the insoluble slag is dried and weighed. The dissolution rate of the uranium product is calculated to be 97.98%. The amount of nitrogen oxides produced during the dissolution process is measured. The analysis results show that almost no nitrogen oxides are produced during the dissolution process of the U3O8 product.
[0041] Example 3
[0042] 100ml of a solution with a nitric acid concentration of 3moL / L is used, the uranium content is calculated at a concentration of 300g / L, the molar ratio of U3O8 to H2O2 products is 1:1, and the uranium content of the U3O8 product is 84.8%, that is, 35.4g of U3O8 product and 4.8g of H2O2 reagent with a content of 30% are added to 100mol of nitric acid solution. The nitric acid solution is heated to 60°C using a water bath thermostatic agitator. Subsequently, the H2O2 reagent is pre-added to the nitric acid solution, mixed evenly, and then the U3O8 product is added. The stirring and dissolving time is 30min. During the dissolution process, the gas is collected and analyzed. After dissolution, the solution is filtered and the insoluble slag is dried and weighed. The dissolution rate of the uranium product is calculated to be 96.83%. The amount of nitrogen oxides produced during the dissolution process is determined to be 99% less than that of the U3O8 product dissolved without adding the H2O2 reagent.
[0043] Example 4
[0044] 100ml of a solution with a nitric acid concentration of 3moL / L is used, the uranium content is calculated at a concentration of 300g / L, the molar ratio of U3O8 to H2O2 products is 1:1.1, and the uranium content of the U3O8 product is 84.8%, that is, 35.4g of U3O8 product and 5.2g of H2O2 reagent with a content of 30% are added to 100mol of nitric acid solution. The nitric acid solution is heated to 50°C using a water bath thermostatic agitator. Subsequently, the H2O2 reagent is pre-added to the nitric acid solution, mixed evenly, and then the U3O8 product is added. The stirring and dissolving time is 60min. During the dissolution process, the gas is collected and analyzed. After dissolution, the solution is filtered and the insoluble slag is dried and weighed. The dissolution rate of the uranium product is calculated to be 96.78%. The amount of nitrogen oxides produced during the dissolution process is measured. The analysis results show that almost no nitrogen oxides are produced during the dissolution process of the U3O8 product.
[0045] Example 5
[0046] 100ml of a solution with a nitric acid concentration of 2.6mol / L is used, the uranium content is calculated at a concentration of 300g / L, the molar ratio of U3O8 to H2O2 products is 1:1.1, and the uranium content of the U3O8 product is 84.8%, that is, 35.4g of U3O8 product and 5.2g of H2O2 reagent with a content of 30% are added to 100mol of nitric acid solution. The nitric acid solution is heated to 60°C using a water bath thermostatic agitator. Subsequently, the H2O2 reagent is pre-added to the nitric acid solution, mixed evenly, and then the U3O8 product is added. The stirring and dissolving time is 60min. During the dissolution process, the gas is collected and analyzed. After dissolution, the solution is filtered and the insoluble slag is dried and weighed. The dissolution rate of the uranium product is calculated to be 96.13%. The amount of nitrogen oxides produced during the dissolution process is measured. The analysis results show that almost no nitrogen oxides are produced during the dissolution process of the U3O8 product.
[0047] The above embodiments are only used to help understand the method and core idea of the present invention. It should be noted that, for those skilled in the art, several improvements and modifications can be made to the present invention without departing from the principles of the present invention, and these improvements and modifications also fall within the scope of protection of the claims of the present invention.
[0048] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A method for solving the problem of nitrogen oxides produced during the nitric acid dissolution process of uranium trioxide products. It is characterized in that The following steps are involved: Heat the nitric acid solution, then add hydrogen peroxide, mix well, add the uranium trioxide product, and stir to dissolve; The molar ratio of uranium trioxide product to hydrogen peroxide is less than or equal to 1; The concentration of nitric acid solution is not less than 2.6 mol / L.
2. The method for solving the problem of nitrogen oxides generated during the nitric acid dissolution process of uranium trioxide product according to claim 1, It is characterized in that The heating temperature is not higher than 60°C.
3. The method for solving the problem of nitrogen oxides generated during the nitric acid dissolution process of uranium trioxide product according to claim 1, It is characterized in that The stirring and dissolving time is not less than 15 minutes.
4. The method for solving the problem of nitrogen oxides generated during the nitric acid dissolution process of uranium trioxide product according to claim 1, It is characterized in that The concentration of the nitric acid solution is 3-6 mol / L.
5. The method for solving the problem of nitrogen oxides generated during the nitric acid dissolution process of uranium trioxide product according to claim 1, It is characterized in that The uranium content of the uranium trioxide product is 84.8%.
Citation Information
Patent Citations
Aqueous-phase preparation method of anhydrous uranyl chloride
CN113772733A