A carbon dioxide-based multi-polymer modified with naphthalene anhydride and a preparation method thereof

By introducing naphthalene ring structure into carbon dioxide-based multi-composites to form planar molecular chains, the problem of insufficient barrier properties of existing degradable plastics is solved, the barrier properties and temperature resistance are significantly improved, and biodegradability is maintained. Suitable for areas with higher barrier requirements.

CN116355189BActive Publication Date: 2024-11-05SHANDONG LECSIN GREEN TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310310518.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-28
Publication Date
2024-11-05
Estimated Expiration
2043-03-28

AI Technical Summary

Technical Problem

Existing biodegradable plastics have shortcomings in barrier properties, especially in areas with higher barrier properties, which cannot meet the needs, and non-degradable plastics can cause environmental pollution.

Method used

Naphthalene ring structure is introduced into the carbon dioxide-based multi-combined copolymer to form quaternary or five-membered random or block copolymers, forming a tiling effect through planar molecular chains to improve barrier properties and temperature resistance.

Benefits of technology

The barrier properties and temperature resistance of the material are significantly improved. The water vapor transmittance at 23℃ is reduced to 0.7g/(m²·24h), and the oxygen transmittance is reduced to 1.3cm³/(m²·24h·0.1MPa), and maintained Biodegradability and avoid environmental pollution.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

A carbon dioxide-based multi-polymer modified with naphthalene anhydride and a preparation method thereof belong to the technical field of degradable plastics. The invention is characterized in that it is a random or block tetrapolymer of propylene oxide, phthalic anhydride, naphthalene anhydride and carbon dioxide, and the preparation steps are as follows: the materials are mixed and added into a reactor, and a catalyst is added; carbon dioxide is charged to carry out a four-membered ring-opening copolymerization reaction; after the reaction is completed, washing, devolatilization, granulation and drying are performed to obtain a purified tetrapolymer. The invention introduces a naphthalene ring structure into the carbon dioxide-based multi-polymer, and an appropriate amount of the naphthalene ring structure further improves the barrier property of the polymer, and the introduction of the naphthalene ring structure also improves the temperature resistance of the carbon dioxide-based multi-polymer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention discloses a carbon dioxide-based multi-polymer modified with naphthalene anhydride and a preparation method thereof, belonging to the technical field of degradable plastics. Background Art

[0002] Currently, the commonly used high barrier plastics are polyvinylidene chloride (PVDC) and ethylene-vinyl alcohol copolymer (EVOH). Among them, PVDC has high water resistance, with a water vapor transmission rate of 0.1g / (m 2 ﹒ 24h)~1g / (m 2 ﹒ 24h), but there is a problem of poor processing performance; EVOH has high oxygen barrier properties, and the oxygen permeability is 0.1cm 3 / (m 2 ﹒ 24h﹒ 0.1MPa)~1cm 3 / (m 2 ﹒ 24h﹒ 0.1MPa), but the water barrier is poor; and PVDC and EVOH are non-degradable, and their large-scale use will cause environmental pollution.

[0003] Polypropylene carbonate (PPC) produced by the copolymerization of propylene oxide and carbon dioxide is a transparent, fully biodegradable binary copolymer with strong barrier properties and a water vapor transmission rate of less than 36g / (m 2 ﹒ 24h), oxygen transmission rate at 23℃ is lower than 108cm 3 / (m 2 ﹒ 24h﹒ 0.1MPa). Based on PPC, the third monomer phthalic anhydride is introduced. The propylene oxide, phthalic anhydride and carbon dioxide ternary copolymer formed by propylene phthalate-propylene carbonate copolymer (PPCP) can not only ensure the transparency and biodegradability of the material without reducing, but also further improve the barrier property. The water vapor transmission rate at 23℃ is 1.2g / (m 2 ﹒ 24h) or less, oxygen transmission rate at 23℃ at 2.5cm 3 / (m 2 ﹒ 24h﹒ 0.1MPa) or less. PPCP is currently the best biodegradable plastic with the best barrier properties. Its water barrier properties are close to PVDC, and its oxygen barrier properties are close to EVOH. It is also biodegradable and will not cause environmental pollution. However, in some areas with higher barrier properties requirements, the barrier properties of PPCP are still slightly insufficient. Summary of the invention

[0004] The technical problem to be solved by the present invention is to overcome the deficiencies of the prior art and provide a carbon dioxide-based multi-polymer modified with naphthalene anhydride and a preparation method thereof which can further improve the barrier properties of the material.

[0005] The technical solution adopted by the present invention to solve the technical problem is: the carbon dioxide-based multi-polymer modified by naphthalene anhydride is characterized by being a tetra- or penta-random or block copolymer of alkylene oxide, phthalic anhydride, naphthalene anhydride and carbon dioxide.

[0006] The present invention introduces a naphthalene ring structure into the carbon dioxide-based multi-polymer, which can further improve the barrier property and temperature resistance of the polymer.

[0007] The general structural formula of the random or block copolymer of the carbon dioxide-based multi-polymer modified by naphthalene anhydride is:

[0008] ;

[0009] Among them, Ar1 and Ar2 are phenyl or naphthyl respectively, and Ar1 and Ar2 are different; R1, R2, and R3 are -H or an alkyl group with less than 6 carbon atoms respectively, and R1 and R3 can form a four-membered ring, a five-membered ring, or a six-membered ring with the main chain; 1≤a≤10000, 1≤b≤10000, 0≤c≤20000, 0≤d≤20000, 1≤c+d≤20000, 0≤e≤1000, 0≤f≤1000, 0≤e≤1000, 1≤c+e, and a, b, c, d, e, f, and g are all integers.

[0010] The present invention introduces a naphthalene ring structure into the carbon dioxide-based multi-polymer. An appropriate amount of the naphthalene ring structure can cause the molecular chain to be in a plane. This planar molecular chain can form a flattening effect, thereby further improving the barrier property of the polymer and making the water vapor permeability at 23°C within 0.7g / (m 2 ﹒ 24h) or less, oxygen transmission rate at 23℃ is 1.3cm 3 / (m 2 ﹒ 24h﹒ 0.1MPa) or less. At the same time, the introduction of naphthalene ring structure can also improve the heat resistance of carbon dioxide-based multi-polymers.

[0011] Preferably, in the above general structural formula:

[0012] 3000≤a≤10000,300≤b+c≤1200,1500≤d≤5000,0≤e≤300.

[0013] Under the optimal ratio between the segments, the barrier properties and heat resistance of the material are better.

[0014] A method for preparing the above-mentioned carbon dioxide-based multi-polymer modified with naphthalene anhydride, the preparation steps are:

[0015] 1) alkylene oxide, phthalic anhydride and naphthalene anhydride are mixed and added into a reaction kettle, and a catalyst is added; the molar ratio of alkylene oxide to phthalic anhydride is 4-10:1; the molar ratio of propylene oxide to naphthalene anhydride is 70-350:1; the molar ratio of alkylene oxide to catalyst is 600-1400:1;

[0016] 2) The injection pressure of carbon dioxide is 0.1MPa~4MPa, and the reaction temperature is heated to 30℃~100℃ for ring-opening copolymerization, and the reaction time is controlled to be 3h~20h; after the reaction, the purified copolymer is obtained by washing, devolatilization, granulation and drying.

[0017] The introduction of naphthalene anhydride can certainly improve the barrier property and temperature resistance of carbon dioxide-based multi-polymer, but naphthalene anhydride will also have greater steric hindrance during polymerization in the synthesis process. Thus it will be more difficult to obtain a copolymer with a large molecular weight. The present invention mainly promotes naphthalene anhydride to participate in polymerization by material matching. The material ratio is based on alkylene oxide, and phthalic anhydride and naphthalene anhydride of appropriate proportion are matched. The structural similarity of phthalic anhydride and naphthalene anhydride is utilized to promote naphthalene anhydride to participate in copolymerization, thereby obtaining a carbon dioxide-based multi-polymer with high naphthalene anhydride copolymer content and high polymerization degree. Under the polymerization process of the present invention, naphthalene anhydride is conducive to participating in copolymerization, and the mass percentage of the copolymer that meets the above-mentioned structural formula in the product after polymerization reaches more than 93%.

[0018] Traditional metal catalysts and non-metal catalysts can meet the basic catalytic requirements of the present invention. In step 1), the catalyst is preferably a composite catalyst formed by the coordination of a non-metal catalyst and a Lewis acid / base pair. In the present invention, non-metal catalysts are preferably used: Lewis acid / base pairs do not introduce metal impurities.

[0019] In the composite catalyst formed by the Lewis acid / base pair described in step 1), the Lewis acid is triethylboron, tributylboron or / and di(trimethylphenyl)boron fluoride, and the Lewis base is one or more of tetra-n-butylammonium fluoride, tetra-n-butylammonium chloride, tetra-n-butylammonium bromide, tetra-n-butylammonium iodide or bis(triphenylphosphorane)ammonium chloride. The above specific Lewis acid / base pair compatibility can meet the catalytic requirements of the present invention and promote the copolymerization of naphthalene anhydride.

[0020] Preferably, the method for preparing the carbon dioxide-based multi-polymer modified with naphthalene anhydride is characterized in that the catalyst described in step 1) is a composite catalyst of tetra-n-butylammonium halide or / and tetra-n-propylammonium halide and triethyl boron or / and tributyl boron. The preferred composite catalyst has a more ideal catalytic effect for the present invention, and the obtained copolymer has a higher content of naphthalene anhydride and better material barrier properties. More preferably, the catalyst described in step 1) is a composite catalyst of triethyl boron and tetra-n-butylammonium halide in a mass ratio of (2~2.5):1.

[0021] Preferably, the method for preparing the carbon dioxide-based multi-polymer modified with naphthalene anhydride is characterized in that: the naphthalene anhydride described in step 1) is 1,8-naphthalene dicarboxylic anhydride and / or 2,3-naphthalene dicarboxylic anhydride. Both naphthalene dicarboxylic anhydride can significantly improve the barrier properties of the copolymer after participating in the copolymerization. 1,8-naphthalene dicarboxylic anhydride is preferred. First, 1,8-naphthalene dicarboxylic anhydride is easier to participate in the copolymerization in the present invention, and it is easy to obtain a carbon dioxide-based copolymer with a higher naphthalene dicarboxylic anhydride content and better barrier properties; second, after 1,8-naphthalene dicarboxylic anhydride participates in the copolymerization, the molecular chain can form a paving effect, and when naphthalene dicarboxylic anhydride with similar content is copolymerized, better barrier properties are exhibited.

[0022] Preferably, the method for preparing the carbon dioxide-based multi-polymer modified with naphthalene anhydride is characterized in that the molar ratio of the alkylene oxide to phthalic anhydride in step 1) is 6 to 8:1.

[0023] Preferably, the method for preparing the carbon dioxide-based multi-polymer modified by naphthalene anhydride is characterized in that the molar feed ratio of the alkylene oxide to the naphthalene anhydride in step 1) is 120-260:1.

[0024] Under the optimal material ratio, which is adapted to the copolymerization participation rate of phthalic acid and phthalic anhydride, the utilization rate of the materials can be improved and the workload of subsequent washing and devolatilization can be reduced.

[0025] Preferably, the method for preparing the carbon dioxide-based multi-polymer modified by naphthalene anhydride is characterized in that the molar ratio of the alkylene oxide to the catalyst in step 1) is 800-1000:1.

[0026] Preferably, the method for preparing the carbon dioxide-based multi-polymer modified by naphthalene anhydride is characterized in that the carbon dioxide charging pressure in step 2) is 2.9MPa~3.8MPa, the reaction temperature is 30℃~45℃, and the reaction time is 4h~9h.

[0027] Under the optimal catalyst dosage and process conditions, the controlled reaction rate can better ensure that naphthalene anhydride participates in the copolymerization and increase the naphthalene anhydride content of the copolymer. The process conditions are preferably low temperature and high pressure, which promotes the participation of carbon dioxide in the copolymerization and forms more space for naphthalene anhydride, which is conducive to the participation of naphthalene anhydride in the copolymerization.

[0028] Compared with the prior art, the carbon dioxide-based multi-polymer modified with naphthalene anhydride and the preparation method thereof of the present invention have the following beneficial effects: the present invention mainly promotes the participation of naphthalene anhydride in polymerization by material matching, the material ratio is based on alkylene oxide, and phthalic anhydride and naphthalene anhydride of appropriate ratio are matched, and the structural similarity of phthalic anhydride and naphthalene anhydride is utilized to promote the participation of naphthalene anhydride in copolymerization, thereby obtaining a carbon dioxide-based multi-polymer with high naphthalene anhydride copolymer content and high polymerization degree. The present invention introduces a naphthalene ring structure into the carbon dioxide-based multi-polymer, and an appropriate amount of the naphthalene ring structure can promote the molecular chain to be in a plane, and this planar molecular chain can form a paving effect, thereby further improving the barrier property of the polymer, and the introduction of the naphthalene ring structure can also improve the temperature resistance of the carbon dioxide-based multi-polymer. DETAILED DESCRIPTION

[0029] The present invention is described in detail below by way of examples. Unless otherwise specified, all raw materials used are commercially available.

[0030] Example 1

[0031] 1) In a dry kettle, high-purity carbon dioxide is used to replace the air in the kettle and then the materials are added. Propylene oxide, phthalic anhydride and 1,8-naphthalic anhydride are mixed and added into the reaction kettle. A catalyst and tetrahydrofuran solvent are also added. The catalyst is a composite catalyst of tetra-n-butylammonium chloride and triethylboron in a molar ratio of 2:1; the molar ratio of propylene oxide to phthalic anhydride is 7:1; the molar ratio of propylene oxide to 1,8-naphthalic anhydride is 190:1; and the molar ratio of propylene oxide to catalyst is 900:1;

[0032] 2) The carbon dioxide was charged at a pressure of 3.4 MPa and heated to a reaction temperature of 35°C for a quaternary ring-opening copolymerization reaction. The reaction time was controlled to be 7 hours. After the reaction was completed, it was dissolved in dichloromethane, a small amount of acid was added to terminate the reaction, and then precipitated with ethanol. The precipitated solid phase was devolatilized, granulated, dried, and analyzed. n =1.49×10 5 g / mol, PDI=2.26, and the mass percentage of the copolymers conforming to the above structural formula in the tested products reached more than 96%.

[0033] Example 2

[0034] 1) In a dry kettle, high-purity carbon dioxide is used to replace the air in the kettle and then the materials are added. Alkylene oxide, phthalic anhydride and 2,3-naphthalic anhydride are mixed and added into the reaction kettle, and a catalyst and tetrahydrofuran solvent are added. The catalyst is a composite catalyst of tetra-n-butylammonium chloride and triethyl boron in a molar ratio of 2:1; the molar ratio of alkylene oxide to phthalic anhydride is 7:1; the molar ratio of alkylene oxide to 2,3-naphthalic anhydride is 190:1; the molar ratio of alkylene oxide to catalyst is 900:1; the alkylene oxide is a mixture of ethylene oxide and propylene oxide in a molar ratio of 2:1;

[0035] 2) The carbon dioxide was charged at a pressure of 3.4 MPa and heated to a reaction temperature of 35°C for a quaternary ring-opening copolymerization reaction. The reaction time was controlled to be 7 hours. After the reaction was completed, it was dissolved in dichloromethane, a small amount of acid was added to terminate the reaction, and then precipitated with ethanol. The precipitated solid phase was devolatilized, granulated, dried, and analyzed. n =1.46×10 5 g / mol, PDI=2.64, and the mass percentage of the copolymers conforming to the above structural formula in the tested products reached more than 95.6%.

[0036] Example 3

[0037] 1) In a dry kettle, high-purity carbon dioxide is used to replace the air in the kettle and then the materials are added. Alkylene oxide, phthalic anhydride and 1,8-naphthalic anhydride are mixed and added into the reaction kettle, and a catalyst and tetrahydrofuran solvent are added. The catalyst is a composite catalyst of tetra-n-butylammonium bromide and triethyl boron in a mass ratio of 2.5:1; the molar ratio of alkylene oxide to phthalic anhydride is 8:1; the molar ratio of alkylene oxide to 1,8-naphthalic anhydride is 260:1; the molar ratio of alkylene oxide to catalyst is 1000:1; the alkylene oxide is a mixture of propylene oxide and cyclohexene oxide in a molar ratio of 4:1;

[0038] 2) The carbon dioxide was charged at a pressure of 3.8 MPa, and the reaction temperature was heated to 45°C for quaternary ring-opening copolymerization, and the reaction time was controlled to be 4 hours; after the reaction was completed, it was dissolved with dichloromethane, a small amount of acid was added to terminate the reaction, and then precipitated with ethanol, the precipitated solid phase was devolatilized, granulated, dried and analyzed, M n =1.48×10 5 g / mol, PDI=2.63, and the mass percentage of the copolymers conforming to the above structural formula in the tested products reached more than 95.4%.

[0039] Example 4

[0040] 1) In a dry kettle, high-purity carbon dioxide is used to replace the air in the kettle and then the materials are added. Propylene oxide, phthalic anhydride and 1,8-naphthalic anhydride are mixed and added into the reaction kettle. A catalyst and tetrahydrofuran solvent are also added. The catalyst is a composite catalyst of tetra-n-butylammonium fluoride and triethylboron in a molar ratio of 2.3:1; the molar ratio of propylene oxide to phthalic anhydride is 6:1; the molar ratio of propylene oxide to 1,8-naphthalic anhydride is 120:1; and the molar ratio of propylene oxide to catalyst is 800:1;

[0041] 2) The carbon dioxide was charged at a pressure of 2.9 MPa, and the reaction temperature was heated to 30°C for quaternary ring-opening copolymerization, and the reaction time was controlled to be 9 hours; after the reaction was completed, it was dissolved with dichloromethane, a small amount of acid was added to terminate the reaction, and then precipitated with ethanol, the precipitated solid phase was devolatilized, granulated, dried and analyzed, M n =1.48×10 5 g / mol, PDI=2.41, and the mass percentage of the copolymer conforming to the above structural formula in the tested product is more than 93.8%.

[0042] Example 5

[0043] 1) In a dry kettle, high-purity carbon dioxide is used to replace the air in the kettle and then the materials are added. Propylene oxide, phthalic anhydride and 1,8-naphthalic anhydride are mixed and added into the reaction kettle. A catalyst and tetrahydrofuran solvent are also added. The catalyst is a composite catalyst of tetra-n-propylammonium chloride and tributyl boron in a molar ratio of 3:1; the molar ratio of propylene oxide to phthalic anhydride is 4:1; the molar ratio of propylene oxide to 1,8-naphthalic anhydride is 70:1; and the molar ratio of propylene oxide to catalyst is 1400:1;

[0044] 2) The carbon dioxide was charged at a pressure of 0.1 MPa, and the reaction temperature was heated to 30°C for quaternary ring-opening copolymerization, and the reaction time was controlled to be 20 h. After the reaction was completed, it was dissolved with dichloromethane, a small amount of acid was added to terminate the reaction, and then precipitated with ethanol. The precipitated solid phase was devolatilized, granulated, dried, and analyzed. n =1.44×10 5 g / mol, PDI=2.33, and the mass percentage of the copolymer conforming to the above structural formula in the tested product is more than 93.7%.

[0045] Example 6

[0046] 1) In a dry kettle, high-purity carbon dioxide is used to replace the air in the kettle and then the materials are added. Alkylene oxide, phthalic anhydride and 1,8-naphthalic anhydride are mixed and added into the reaction kettle, and a catalyst and tetrahydrofuran solvent are added. The catalyst is a composite catalyst of tetra-n-propylammonium fluoride and triethyl boron in a molar ratio of 1.5:1; the molar ratio of alkylene oxide to phthalic anhydride is 10:1; the molar ratio of alkylene oxide to 1,8-naphthalic anhydride is 350:1; the molar ratio of alkylene oxide to catalyst is 600:1; the alkylene oxide is a mixture of ethylene oxide and cyclohexene oxide in a molar ratio of 10:1;

[0047] 2) The carbon dioxide was charged at a pressure of 4 MPa and heated to a reaction temperature of 100°C for a quaternary ring-opening copolymerization reaction. The reaction time was controlled to be 3 h. After the reaction was completed, it was dissolved in dichloromethane, a small amount of acid was added to terminate the reaction, and then precipitated with ethanol. The precipitated solid phase was devolatilized, granulated, dried, and analyzed. n =1.42×10 5 g / mol, PDI=2.66, and the mass percentage of the copolymer conforming to the above structural formula in the tested product is more than 93.2%.

[0048] Comparative Example 1

[0049] The material ratio and preparation process of Example 1 were followed, except that the 1,8-naphthalene dicarboxylic anhydride in the material was replaced by phthalic anhydride in the same molar amount; the M n =1.40×10 5 g / mol, PDI=2.27.

[0050] The copolymers obtained in the examples and comparative examples were made into samples for performance testing:

[0051] 1. Water vapor transmission rate is tested according to GB / T 1037, and the film thickness is 80μm.

[0052] 2. Oxygen permeability is tested in accordance with GB / T 1038, with a film thickness of 80 μm.

[0053] The water vapor and oxygen permeabilities of the copolymers prepared in Examples 1 to 3 of the present invention and Comparative Example 1 are compared in the following table:

[0054] Example Glass transition temperature℃ Pyrolysis temperature℃ <![CDATA[Oxygen transmission rate cm 3 / (m 2 ·24 h·0.1 MPa)]]> <![CDATA[Water vapor transmission rate g / (m 2 ·24 h]]> Example 1 83.4 318 1.1 0.4 Example 2 81.2 311 1.2 0.5 Example 3 82.4 316 1.1 0.4 Example 4 82.2 316 1.1 0.5 Example 5 80.6 310 1.2 0.6 Example 6 80.1 305 1.3 0.7 Comparative Example 1 68.4 263 2.0 1.1

[0055] It can be seen that the biodegradable propylene oxide-phthalic anhydride-naphthalic anhydride-carbon dioxide quaternary copolymer prepared by the present invention can significantly improve the barrier properties while ensuring the degradability compared with propylene oxide-phthalic anhydride-carbon dioxide. The present invention can be applied to the modification of PPCP materials and make their application more extensive.

[0056] The above is only a preferred embodiment of the present invention, and does not limit the present invention in other forms. Any technician familiar with the profession may use the above disclosed technical content to change or modify it into an equivalent embodiment with equivalent changes. However, any simple modification, equivalent change and modification made to the above embodiment according to the technical essence of the present invention without departing from the technical solution of the present invention still belongs to the protection scope of the technical solution of the present invention.

Claims

1. A carbon dioxide-based multipolymer modified with naphthalene anhydride, It is characterized in that It is a quaternary random or block copolymer of alkylene oxide, phthalic anhydride, naphthalene anhydride and carbon dioxide; The preparation steps are: 1) mixing alkylene oxide, phthalic anhydride and naphthalene anhydride and adding them into a reaction kettle, and adding a catalyst; the molar ratio of alkylene oxide to phthalic anhydride is 4-10:1; the molar ratio of alkylene oxide to naphthalene anhydride is 70-350:1; the molar ratio of alkylene oxide to catalyst is 600-1400:1; 2) The injection pressure of carbon dioxide is 0.1MPa~4MPa, and the reaction temperature is heated to 30℃~100℃ to carry out the quaternary ring-opening copolymerization reaction, and the reaction time is controlled to be 3h~20h; after the reaction, washing, devolatilization, granulation and drying are carried out to obtain the purified quaternary copolymer.

2. A method for preparing the carbon dioxide-based multi-polymer modified with naphthalene anhydride according to claim 1, It is characterized in that The preparation steps are: 1) mixing alkylene oxide, phthalic anhydride and naphthalene anhydride and adding them into a reaction kettle, and adding a catalyst; the molar ratio of alkylene oxide to phthalic anhydride is 4-10:1; the molar ratio of alkylene oxide to naphthalene anhydride is 70-350:1; the molar ratio of alkylene oxide to catalyst is 600-1400:1; 2) The injection pressure of carbon dioxide is 0.1MPa~4MPa, and the reaction temperature is heated to 30℃~100℃ to carry out the quaternary ring-opening copolymerization reaction, and the reaction time is controlled to be 3h~20h; after the reaction, washing, devolatilization, granulation and drying are carried out to obtain the purified quaternary copolymer.

3. The method for preparing a carbon dioxide-based multipolymer modified with naphthalene anhydride according to claim 2, Features: The catalyst in step 1) is a composite catalyst of tetra-n-butylammonium halide or / and tetra-n-propylammonium halide and triethylboron or / and tributylboron.

4. The method for preparing a carbon dioxide-based multi-polymer modified with naphthalene anhydride according to claim 2, Features: The naphthalene anhydride in step 1) is 1,8-naphthalene dicarboxylic anhydride or / and 2,3-naphthalene dicarboxylic anhydride.

5. The method for preparing a carbon dioxide-based multi-polymer modified with naphthalene anhydride according to claim 2, Features: The molar ratio of the alkylene oxide to phthalic anhydride in step 1) is 6-8:

1.

6. The method for preparing a carbon dioxide-based multi-polymer modified with naphthalene anhydride according to claim 2, Features: The molar feed ratio of the alkylene oxide to the naphthalene anhydride in step 1) is 120-260:

1.

7. The method for preparing a carbon dioxide-based multi-polymer modified with naphthalene anhydride according to claim 2, Features: The molar ratio of the alkylene oxide to the catalyst in step 1) is 800-1000:

1.

8. The method for preparing a carbon dioxide-based multi-polymer modified with naphthalene anhydride according to claim 2, Features: The carbon dioxide charging pressure in step 2) is 2.9 MPa to 3.8 MPa, the reaction temperature is 30° C. to 45° C., and the reaction time is 4 h to 9 h.