Lanthanum magnetic iron modified attapulgite adsorbent for phosphorus removal and its application

By loading lanthanum and γ-Fe2O3 on the concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave and concave soil, the problem of poor phosphorus removal effect in the existing technology is solved, and the water body is ≤2mg/L is achieved The efficient phosphorus removal is suitable for pollution control of eutrophication rivers.

CN116371353BActive Publication Date: 2024-11-12GUANGDONG UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310366119.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-06
Publication Date
2024-11-12
Estimated Expiration
2043-04-06

AI Technical Summary

Technical Problem

The existing magnetic lanthanum-loaded concave and concave rock stone clay phosphorus removal adsorbent has poor phosphorus removal effect in water bodies with a phosphorus concentration of ≤2mg/L, and cannot effectively remove low-concentration phosphorus.

Method used

By loading lanthanum and γ-Fe2O3 on the concave and convex rod soil, calcining at 650-750°C and aging process of 20-26 hours, the pH is adjusted to 10-11, and phosphorus removal adsorbent of lanthanum magnetic iron modified concave and convex rod soil is prepared. Increase its specific surface area and adsorption active sites to improve the removal ability of low-concentration phosphorus.

Benefits of technology

It significantly improves the removal effect of low concentration phosphorus of ≤2mg/L, solves the problem of poor phosphorus removal effect in the prior art, and is suitable for water bodies with phosphorus concentration ≤2mg/L, especially in the pollution control of eutrophication rivers. Have good results.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116371353B_ABST
    Figure CN116371353B_ABST
Patent Text Reader

Abstract

The invention discloses a lanthanum magnetic iron modified attapulgite dephosphorization adsorbent and an application thereof. The lanthanum magnetic iron modified attapulgite dephosphorization adsorbent comprises attapulgite, on which lanthanum and γ-Fe2O3 are loaded; a preparation method of the lanthanum magnetic iron modified attapulgite dephosphorization adsorbent comprises the following steps: attapulgite calcined at 650-750 DEG C reacts with a divalent iron salt and a trivalent iron salt, heats, adjusts the pH to 10-11, and simultaneously adds a lanthanum salt, ages for 20-26 hours, washes with anhydrous ethanol and water, separates, and dries to obtain the lanthanum magnetic iron modified attapulgite dephosphorization adsorbent; the mass ratio of the lanthanum salt, the calcined attapulgite, the divalent iron salt and the trivalent iron salt is 1:(1.5-2.5):(0.5-1.5):(0.5-1.5). The lanthanum magnetic iron modified attapulgite phosphorus removal adsorbent has a large specific surface area and many adsorption active sites, and has a good phosphorus removal effect on low concentration phosphorus of ≤2 mg / L.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of phosphorus removal adsorbents, and in particular relates to a lanthanum magnetic iron modified attapulgite phosphorus removal adsorbent and application thereof. Background Art

[0002] Eutrophication of water bodies is a common water pollution problem, and nitrogen and phosphorus are the main pollutants that cause eutrophication of water bodies. Studies have shown that when the N / P ratio is low, it is conducive to the formation of algae in water bodies. Nitrogen can be removed from water bodies through nitrogen fixation, while phosphorus cannot be circulated in nature and will continue to accumulate in water bodies and sediments. When the total phosphorus concentration is greater than 0.02 mg / L, it will cause eutrophication of water bodies, so it is very necessary to control the total phosphorus concentration in water bodies.

[0003] Common phosphorus removal methods include biological method, chemical precipitation method, ion exchange resin method and adsorption method. For the effluent of sewage treatment plants and eutrophic river water bodies, the phosphorus concentration is usually below 1 mg / L, and the maximum does not exceed 2 mg / L. For the removal of such low-concentration phosphorus, both biological method and chemical precipitation method are not effective, and the equipment structure of the resin method is complex and the operation process is long. Compared with other phosphorus removal methods, the adsorption method has the advantages of simple operation, low energy consumption, high efficiency and stable operation.

[0004] Attapulgite is a kind of silicate mineral clay rich in magnesium and aluminum, composed of nano-rod-shaped silicate crystals. Attapulgite is highly hydrophilic, plastic in water, rich in surface active groups, has strong cohesive adhesion between molecules, and has a large specific surface area. However, natural attapulgite is not effective in phosphorus removal due to its low adsorption capacity, so it often needs to be modified when removing phosphorus. For example, there is a Chinese patent that prepares a magnetic lanthanum-loaded attapulgite clay dephosphorization adsorbent by loading lanthanum and ferroferric oxide on a attapulgite clay carrier, and uses it to eliminate phosphorus pollution. However, the inventor found in preliminary research that for water bodies with a phosphorus concentration of ≤2mg / L, the magnetic lanthanum-loaded attapulgite clay dephosphorization adsorbent has a poor dephosphorization effect.

[0005] Therefore, it is of great economic value and significance to develop a lanthanum magnetic iron modified attapulgite phosphorus removal adsorbent that has a high efficiency in removing phosphorus at low concentrations of ≤2 mg / L. Summary of the invention

[0006] The primary purpose of the present invention is to solve the problem that the existing magnetic lanthanum-loaded attapulgite clay phosphorus removal adsorbent has poor removal effect on low-concentration phosphorus of ≤2 mg / L, and to provide a lanthanum magnetic iron-modified attapulgite clay phosphorus removal adsorbent.

[0007] Another object of the present invention is to provide the use of lanthanum magnetic iron modified attapulgite phosphorus removal adsorbent in water bodies with phosphorus concentration ≤ 2 mg / L.

[0008] In order to achieve the above object, the present invention adopts the following technical solutions:

[0009] Lanthanum magnetic iron modified attapulgite phosphorus removal adsorbent, comprising attapulgite, lanthanum and γ-Fe loaded on the attapulgite 2 O 3 The preparation method of the lanthanum magnetic iron modified attapulgite phosphorus removal adsorbent comprises the following steps:

[0010] The attapulgite calcined at 650-750° C. is reacted with a divalent iron salt and a trivalent iron salt, heated, the pH is adjusted to 10-11, and a lanthanum salt is added at the same time, aged for 20-26 hours, washed with anhydrous ethanol and water, separated, and dried to obtain a lanthanum magnetic iron modified attapulgite phosphorus removal adsorbent;

[0011] The mass ratio of the lanthanum salt, the calcined attapulgite, the divalent iron salt and the trivalent iron salt is 1:(1.5-2.5):(0.5-1.5):(0.5-1.5).

[0012] Compared with the loading of lanthanum and ferroferric oxide, the loading of lanthanum and γ-Fe 2 O 3 The attapulgite has a larger specific surface area and more adsorption active sites, which is more suitable for removing low-concentration phosphorus and has a good phosphorus removal effect on low-concentration phosphorus ≤2 mg / L.

[0013] Compared with the attapulgite calcined at low temperature (temperature below 650°C), the attapulgite calcined at high temperature of 650-750°C has the ability to induce the reaction of divalent iron salt and trivalent iron salt to generate γ-Fe 2 O 3 At the same time, the attapulgite calcined at 650-750℃ needs to be aged for 20-26h to exert its ability to induce the reaction of divalent iron salt and trivalent iron salt to generate γ-Fe 2 O 3 The ability to obtain γ-Fe 2 O 3 And lanthanum compounds and lanthanide with stable structure of lanthanum magnetic iron modified attapulgite phosphorus removal adsorbent. And if the aging time is too short, not only can γ-Fe 2 O 3 At the same time, the structure of the lanthanum magnetic iron modified attapulgite phosphorus removal adsorbent will be unstable, thereby reducing the adsorption effect of the lanthanum magnetic iron modified attapulgite phosphorus removal adsorbent on low concentration phosphorus of ≤2 mg / L.

[0014] When the mass ratio of lanthanum salt, calcined attapulgite, divalent iron salt and trivalent iron salt is in the range of 1:(1.5-2.5):(0.5-1.5):(0.5-1.5), the lanthanum magnetic iron modified attapulgite phosphorus removal adsorbent will have a larger specific surface area and more active sites, and has a stronger phosphorus removal effect, and has a better phosphorus removal effect on low-concentration phosphorus of ≤2 mg / L.

[0015] In addition, the preparation method of the lanthanum magnetic iron modified attapulgite phosphorus removal adsorbent of the present invention adjusts the pH to 10-11 because when the pH is 10-11, it is beneficial for lanthanum and γ-Fe 2 O 3 Sedimented on the surface of attapulgite.

[0016] Specifically, the pH adjusting agent for adjusting the pH is one or more of sodium hydroxide, ammonia water, hydrochloric acid or sulfuric acid.

[0017] When using the pH adjuster, it should be added slowly under stirring conditions to avoid local overconcentration and the formation of an oversaturated solution, which will affect the preparation of the lanthanum magnetic iron modified attapulgite phosphorus removal adsorbent.

[0018] The purpose of adding anhydrous ethanol for washing is to reduce the γ-Fe 2 O 3 The agglomeration of lanthanum magnetic iron modified attapulgite phosphorus removal adsorbent is generated with a more uniform structure, thereby improving the phosphorus removal effect of the lanthanum magnetic iron modified attapulgite phosphorus removal adsorbent.

[0019] Specifically, the lanthanum salt is at least one of lanthanum nitrate or lanthanum chloride.

[0020] Preferably, the lanthanum chloride is lanthanum chloride hexahydrate.

[0021] Specifically, the divalent iron salt is one or more of ferrous sulfate heptahydrate, ferrous chloride, anhydrous ferrous sulfate or ferrous nitrate.

[0022] Specifically, the trivalent iron salt is one or more of ferric chloride, ferric sulfate or ferric nitrate.

[0023] Specifically, the divalent iron salt and the trivalent iron salt are dissolved in water to prepare a mixed iron solution before use.

[0024] Specifically, the calcination time is 4 to 6 hours.

[0025] Specifically, the heating temperature is 70-85°C.

[0026] Specifically, the drying temperature is 60-75°C.

[0027] Specifically, the drying time is 9 to 17 hours.

[0028] The small particle size of the lanthanum magnetic iron modified attapulgite phosphorus removal adsorbent can increase the specific surface area of ​​the lanthanum magnetic iron modified attapulgite phosphorus removal adsorbent, making it easier to fully contact with pollutants such as phosphorus, thereby improving the phosphorus removal effect of the lanthanum magnetic iron modified attapulgite phosphorus removal adsorbent.

[0029] Specifically, the particle size of the lanthanum magnetic iron modified attapulgite phosphorus removal adsorbent is ≤0.075 mm.

[0030] The use of the above-mentioned lanthanum magnetic iron modified attapulgite phosphorus removal adsorbent in water bodies with phosphorus concentration ≤ 2 mg / L should also be within the protection scope of the present invention.

[0031] Preferably, the lanthanum magnetic iron modified attapulgite phosphorus removal adsorbent is used in water bodies with phosphorus concentrations ≥1.0 mg / L and ≤2 mg / L.

[0032] The phosphorus concentration in the present invention refers to the phosphate concentration.

[0033] The phosphorus in the low concentration phosphorus of the present invention refers to phosphate.

[0034] Compared with the prior art, the present invention has the following beneficial effects:

[0035] The lanthanum magnetic iron modified attapulgite phosphorus removal adsorbent of the present invention is composed of attapulgite loaded with lanthanum and γ-Fe 2 O 3 Compared with the loading of lanthanum and ferroferric oxide, the loading of lanthanum and γ-Fe 2 O 3 The lanthanum magnetic iron modified attapulgite phosphorus removal adsorbent has a larger specific surface area and more adsorption active sites, and is more suitable for removing low-concentration phosphorus. It has a good phosphorus removal effect on low-concentration phosphorus of ≤2 mg / L, solving the problem that the existing magnetic lanthanum loaded attapulgite clay phosphorus removal adsorbent has poor removal effect on low-concentration phosphorus of ≤2 mg / L. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 The XRD diagrams of the lanthanum magnetic iron modified attapulgite phosphorus removal adsorbents of Example 1 and Comparative Examples 1-2 are shown.

[0037] Figure 2 This is a scatter plot of the relationship between the phosphate adsorption amount and adsorption time of the lanthanum magnetic iron modified attapulgite phosphorus removal adsorbent in Example 1. DETAILED DESCRIPTION

[0038] The present invention is further described below in conjunction with examples. These examples are only used to illustrate the present invention and are not intended to limit the scope of the present invention. The experimental methods in the following examples that do not specify specific conditions are usually carried out according to conventional conditions in the art or according to the conditions recommended by the manufacturer; the raw materials, reagents, etc. used, unless otherwise specified, are all raw materials and reagents that can be obtained from commercial channels such as conventional markets. Any non-substantial changes and substitutions made by those skilled in the art on the basis of the present invention belong to the scope of protection claimed by the present invention.

[0039] Example 1

[0040] This embodiment provides a lanthanum magnetic iron modified attapulgite phosphorus removal adsorbent, including attapulgite, lanthanum and γ-Fe are loaded on the attapulgite 2 O 3 The preparation method of the lanthanum magnetic iron modified attapulgite phosphorus removal adsorbent comprises the following steps:

[0041] S1. Pass the attapulgite through a 200-mesh sieve, place it in a muffle furnace, and calcine it at 700°C for 5h for later use;

[0042] S2. Dissolve 5g of ferrous sulfate heptahydrate and 5g of ferric chloride in 200ml of deionized water, ultrasonicate for 0.5h to prepare a mixed iron solution, add 10g of attapulgite calcined in step S1, mix thoroughly, stir for 1h, heat to 75°C, slowly add 0.1mol / L sodium hydroxide under stirring to adjust the pH to 11, and simultaneously add 5g of lanthanum chloride hexahydrate, continue stirring for 4h, age for 24h, wash with anhydrous ethanol and distilled water for multiple times and separate, collect the precipitate with a magnet, dry in an oven at 65°C for 12h, grind, and obtain a lanthanum magnetic iron modified attapulgite phosphorus removal adsorbent, whose XRD pattern is shown as follows: Figure 1 As shown, the particle size of the lanthanum magnetic iron modified attapulgite phosphorus removal adsorbent is ≤0.075mm;

[0043] The mass ratio of the lanthanum chloride hexahydrate, the calcined attapulgite, the ferrous sulfate heptahydrate and the ferric chloride is 1:2:1:1.

[0044] Examples 2 to 3 and Comparative Example 1

[0045] Examples 2 to 3 and Comparative Example 1 provide lanthanum magnetic iron modified attapulgite phosphorus removal adsorbents, which differ from Example 1 only in the aging time, and the rest are consistent with Example 1, specifically:

[0046] Table 1 Aging time of Examples 1 to 3 and Comparative Example 1

[0047] Aging time / h Example 1 24 Example 2 20 Example 3 26 Comparative Example 1 0.5

[0048] Embodiment 4-5

[0049] Examples 4 to 5 provide lanthanum magnetic iron modified attapulgite phosphorus removal adsorbents, which differ from Example 1 only in that the mass ratios of lanthanum chloride hexahydrate, calcined attapulgite, ferrous sulfate heptahydrate and ferric chloride are different, and the rest are consistent with Example 1, specifically:

[0050] Table 2 Mass ratio of lanthanum chloride hexahydrate, calcined attapulgite, ferrous sulfate heptahydrate and ferric chloride in Examples 1, 4 to 5

[0051]

[0052] Embodiment 6-7

[0053] Examples 6 to 7 provide lanthanum magnetic iron modified attapulgite phosphorus removal adsorbents, which differ from Example 1 only in the calcination temperature in step S1, and the rest are consistent with Example 1, specifically:

[0054] Table 3 Calcination temperature in step S1 of Examples 1, 6-7

[0055] Calcination temperature / ℃ Example 1 700 Example 6 650 Example 7 750 Comparative Example 2 450

[0056] Comparative Example 3

[0057] The comparative example provides a magnetic lanthanum-loaded attapulgite clay dephosphorus adsorbent, comprising an attapulgite clay carrier, on which lanthanum and ferrosoferric oxide are loaded.

[0058] The preparation method of the magnetic lanthanum-loaded attapulgite clay phosphorus removal adsorbent refers to Example 1 of Chinese patent CN113145063A.

[0059] Comparative Example 4

[0060] This comparative example provides a magnetic iron-modified attapulgite phosphorus removal adsorbent, comprising attapulgite, on which γ-Fe is loaded. 2 O 3 ; The only difference from Example 1 is that 5g of lanthanum chloride hexahydrate is not added.

[0061] Comparative Example 5

[0062] This comparative example provides a lanthanum-modified attapulgite phosphorus removal adsorbent, including attapulgite on which lanthanum is loaded; the only difference from Example 1 is that 5g of ferrous sulfate heptahydrate and 5g of ferric chloride are not added.

[0063] Sample characterization

[0064] Figure 1 The XRD diagrams of the lanthanum magnetic iron modified attapulgite phosphorus removal adsorbents of Example 1 and Comparative Examples 1-2 are shown in FIG. Figure 1 As shown, the lanthanum magnetic iron modified attapulgite phosphorus removal adsorbent of Example 1 contains γ-Fe2 O 3 In addition, from Figure 1 It can be seen that the lanthanum magnetic iron modified attapulgite phosphorus removal adsorbent of Comparative Examples 1 and 2 does not contain γ-Fe 2 O 3 This fully demonstrates that when the aging time is too short or the calcination temperature of attapulgite is too low, it is not conducive to the formation of γ-Fe 2 O 3 of.

[0065] The lanthanum magnetic iron modified attapulgite phosphorus removal adsorbent of Example 1 was tested by X-ray fluorescence spectrometer (XRF), and the experimental results are shown in Table 4:

[0066] Table 4 XRF test results of lanthanum magnetic iron modified attapulgite phosphorus removal adsorbent in Example 1

[0067]

[0068] From Table 4, we can see that the lanthanum magnetic iron modified attapulgite phosphorus removal adsorbent contains lanthanum element, combined with Figure 1 It can be seen that the lanthanum magnetic iron modified attapulgite phosphorus removal adsorbent of the present invention is loaded with lanthanum and γ-Fe 2 O 3 .

[0069] In addition, the XRD patterns of the lanthanum magnetic iron modified attapulgite phosphorus removal adsorbents in Examples 2 to 7 are similar to those in Example 1. Figure 1 Similarly, the XRF test results of the lanthanum magnetic iron modified attapulgite phosphorus removal adsorbents in Examples 2 to 7 are similar to those in Table 4 of Example 1.

[0070] Performance Testing

[0071] 1. Phosphorus removal experiment with different adsorbents

[0072] (1) At room temperature, dissolve 2 mg of potassium dihydrogen phosphate in 1 L of distilled water to prepare a 2 mg / L phosphate solution, and adjust the solution to pH = 7 with 0.1 mol / L HCl and 0.1 mol / L NaOH.

[0073] (2) 0.8 g of unmodified attapulgite, the adsorbents of each embodiment and each comparative example were taken and respectively put into 1 L of 2 mg / L phosphate solution for full reaction for 24 h. The phosphate concentration C′ in the solution was then measured and the phosphate removal rate was calculated according to the formula: The experimental results are shown in Table 3:

[0074] Table 5 Phosphorus removal effect of low concentration phosphorus

[0075] sample Adsorbent composition Phosphate removal rate / % Example 1 <![CDATA[Attapulgite supported lanthanum and γ-Fe 2 O 3 > 92.67 Comparative Example 1 / 50.00 Comparative Example 2 / 63.20 Comparative Example 3 Attapulgite clay loaded with lanthanum and ferroferric oxide 75.40 Comparative Example 4 <![CDATA[Attapulgite-supported γ-Fe 2 O 3 > 8.10 Comparative Example 5 Attapulgite loaded with lanthanum 74.50 Control group Attapulgite 6.43

[0076] As shown in Table 5, the phosphate removal rate of Comparative Example 1 is much lower than that of Example 1 because the aging time of Comparative Example 1 is too short, only 0.5 h, when preparing the lanthanum magnetic iron modified attapulgite phosphorus removal adsorbent. 2 O 3 At the same time, it will also cause the structure of the lanthanum magnetic iron modified attapulgite phosphorus removal adsorbent to become unstable, thereby reducing the adsorption effect of the lanthanum magnetic iron modified attapulgite phosphorus removal adsorbent on low-concentration phosphorus of ≤2 mg / L, resulting in the lanthanum magnetic iron modified attapulgite phosphorus removal adsorbent in comparative example 1 having a phosphorus removal effect on low-concentration phosphorus of ≤2 mg / L that is far worse than that in Example 1.

[0077] The phosphate removal rate of Comparative Example 2 is much lower than that of Example 1 because the temperature of calcining the attapulgite is too low (lower than 650°C) when preparing the lanthanum magnetic iron modified attapulgite phosphorus removal adsorbent in Comparative Example 2, and the divalent iron salt and the trivalent iron salt cannot be induced to react to generate γ-Fe 2 O 3 ; The attapulgite calcined at 650-750°C in Example 1 has the effect of inducing the reaction of divalent iron salt and trivalent iron salt to generate γ-Fe 2 O 3 Therefore, the lanthanum magnetic iron modified attapulgite phosphorus removal adsorbent prepared in Example 1 contains γ-Fe 2 O 3 It has a better phosphorus removal effect on low-concentration phosphorus of ≤2mg / L.

[0078] The lanthanum magnetic iron modified attapulgite phosphorus removal adsorbent of the present invention has the best phosphorus removal effect on low concentration phosphorus of ≤2mg / L, which is much higher than the magnetic lanthanum loaded attapulgite clay phosphorus removal adsorbent of comparative example 3. This is because compared with the loaded lanthanum and ferroferric oxide, the loaded lanthanum and γ-Fe 2 O 3 The attapulgite has a higher specific surface area and more adsorption active sites, and is more suitable for removing low-concentration phosphorus, and has a better phosphorus removal effect on low-concentration phosphorus of ≤2 mg / L. At the same time, by comparing the data of Example 1, Comparative Examples 4-5 and the control group, it can be seen that lanthanum and γ-Fe 2 O 3 The specific combination is the key to the excellent phosphorus removal effect of the lanthanum magnetic iron modified attapulgite phosphorus removal adsorbent of the present invention on low-concentration phosphorus of ≤2 mg / L.

[0079] In addition, the phosphorus removal effect of the lanthanum magnetic iron modified attapulgite phosphorus removal adsorbent in Examples 2 to 7 on low-concentration phosphorus of ≤2 mg / L is similar to that in Example 1.

[0080] 2. Phosphorus removal experiment of lanthanum magnetic iron modified attapulgite for different low concentration phosphorus

[0081] (1) At room temperature, 0.2, 0.4, 0.6, 0.8, 1.0, 1.2, 1.4, 1.6, 1.8, 2.0, 5.0 and 10.0 mg were dissolved in 1 L of distilled water to make 0.2, 0.4, 0.6, 0.8, 1.0, 1.2, 1.4, 1.6, 1.8, 2.0, 5.0 and 10.0 mg / L phosphate solutions, respectively. The solutions were adjusted to pH 7 with 0.1 mol / L HCl and 0.1 mol / L NaOH.

[0082] (2) Take 0.8 g of the lanthanum magnetic iron modified attapulgite phosphorus removal adsorbent of Example 1 and put it into 1 L of the above phosphate solutions of different concentrations to fully react for 24 hours, then measure the phosphate concentration C' in the solution, and calculate the phosphate removal rate according to the formula: Where A refers to the initial concentration of different phosphate solutions. The experimental results are shown in Table 6:

[0083] Table 6 Example 1 Phosphorus removal effect of lanthanum magnetic iron modified attapulgite on different low concentrations of phosphorus

[0084] Concentration of lanthanum magnetic iron modified attapulgite for phosphorus removal / mg / L Phosphate removal rate / % 0.2 75.49 0.4 76.90 0.6 84.95 0.8 89.52 1.0 90.20 1.2 93.34 1.4 93.30 1.6 93.25 1.8 93.00 2.0 92.67 5.0 92.54 10.0 92.07

[0085] As can be seen from Table 6, the lanthanum magnetic iron modified attapulgite phosphorus removal adsorbent of the present invention has a good phosphorus removal effect on water bodies with a phosphorus concentration of ≤2 mg / L, and in particular, the lanthanum magnetic iron modified attapulgite phosphorus removal adsorbent of the present invention has a good phosphorus removal effect on water bodies with a phosphorus concentration of ≥1.0 mg / L and ≤2 mg / L. Since the phosphorus concentration in eutrophic rivers is mostly ≤2 mg / L, the lanthanum magnetic iron modified attapulgite phosphorus removal adsorbent of the present invention has a good effect on the treatment of low-concentration phosphorus in eutrophic rivers.

[0086] 3. Effect of adsorption time on the phosphorus removal effect of lanthanum magnetic iron modified attapulgite phosphorus removal adsorbent

[0087] 0.8 g of the lanthanum magnetic iron modified attapulgite phosphorus removal adsorbent of Example 1 was put into 1 L of 2 mg / L phosphate solution with a pH of 7 for reaction, and the phosphate concentration C′ in the solution was measured at 0.25 h, 0.75 h, 1 h, 3 h, 6 h, 9 h, 12 h, 18 h and 24 h, respectively, and a scatter plot of the relationship between the phosphate adsorption amount and the adsorption time of the lanthanum magnetic iron modified attapulgite phosphorus removal adsorbent was drawn, as shown in FIG. Figure 2 As shown, the experimental results were fitted with the adsorption pseudo-first-order kinetic equation and the adsorption pseudo-second-order kinetic equation, respectively, and Table 7 was obtained:

[0088] Table 7 Kinetic parameters of phosphate adsorption by lanthanum magnetic iron modified attapulgite phosphorus removal adsorbent

[0089]

[0090] In addition, the phosphate removal rate was calculated according to the formula, The experimental results are shown in Table 8:

[0091] Table 8 Phosphorus removal effect of lanthanum magnetic iron modified attapulgite phosphorus removal adsorbent at different adsorption times

[0092]

[0093] Figure 2 The scatter plot is a relationship between the phosphate adsorption amount and adsorption time of the lanthanum magnetic iron modified attapulgite phosphorus removal adsorbent in Example 1. Figure 2 As shown in Table 7, the adsorption process of phosphate by the lanthanum magnetic iron modified attapulgite phosphorus removal adsorbent of the present invention is divided into two stages, first a rapid adsorption stage and then a slow adsorption stage. When the adsorption time is 0.25h, the adsorption rate of phosphate by the lanthanum magnetic iron modified attapulgite phosphorus removal adsorbent is very fast. When the adsorption time reaches 6h, the phosphate adsorption amount remains almost unchanged, indicating that the adsorption of phosphate by the lanthanum magnetic iron modified attapulgite phosphorus removal adsorbent has reached equilibrium. Moreover, the adsorption kinetics of phosphate by the lanthanum magnetic iron modified attapulgite phosphorus removal adsorbent of the present invention is more in line with the pseudo-secondary kinetic model, and the initial adsorption rate is 3.24g / (mg·h).

[0094] In addition, it can be seen from Table 8 that in the rapid adsorption stage, when the adsorption time is 0.25h, the phosphate removal rate of the lanthanum magnetic iron modified attapulgite phosphorus removal adsorbent of the present invention can quickly reach 75.00%; then with the increase of time, the adsorption of phosphate by the lanthanum magnetic iron modified attapulgite phosphorus removal adsorbent of the present invention gradually reaches equilibrium, and at equilibrium, the phosphate removal rate of the lanthanum magnetic iron modified attapulgite phosphorus removal adsorbent is 92.67%.

[0095] 4. Effect of coexisting ions on the phosphorus removal effect of lanthanum magnetic iron modified attapulgite phosphorus removal adsorbent

[0096] (1) At room temperature, dissolve 2 mg of potassium dihydrogen phosphate in 1 L of distilled water to prepare a 2 mg / L phosphate solution, and adjust the solution to pH = 7 with 0.1 mol / L HCl and 0.1 mol / L NaOH.

[0097] (2) Based on 1L of the phosphate solution prepared in (1), a series of phosphate solutions containing different coexisting ions were prepared as shown in Table 9, and 0.8g of the lanthanum magnetic iron modified attapulgite phosphorus removal adsorbent of Example 1 was added to each solution. The solution was fully reacted for 24h, and then the phosphate concentration C' in the solution was measured. The phosphate removal rate was calculated according to the formula: The experimental results are also shown in Table 9:

[0098] Table 9 Phosphate solutions containing different coexisting ions

[0099]

[0100] Note: No. 1 in the table refers to 1L of 2mg / L phosphate solution at pH=7 without any coexisting ions; No. 2 refers to 1mmol / L Cl - 1L of 2mg / L phosphate solution with pH=7, and so on for numbers 3 to 13.

[0101] From Table 9, we can see that the coexisting ion Cl in the range of 1 to 100 mmol / L - , HCO 3 - 、SO 4 2- and F - None of them will have a significant impact on the phosphorus removal effect of the lanthanum magnetic iron modified attapulgite phosphorus removal adsorbent of the present invention.

[0102] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not intended to limit the embodiments of the present invention. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the embodiments here. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the claims of the present invention.

Claims

1. A method for preparing a lanthanum magnetic iron modified attapulgite phosphorus removal adsorbent, characterized in that: The raw materials include attapulgite, on which lanthanum and γ-Fe2O3 are loaded; the preparation method of the lanthanum magnetic iron modified attapulgite phosphorus removal adsorbent includes the following steps: The attapulgite calcined at 650-750°C reacts with a divalent iron salt and a trivalent iron salt, and is heated to adjust the pH to 10-11, and lanthanum salt is added at the same time, aged for 20-26 hours, washed with anhydrous ethanol and water, separated, and dried to obtain a lanthanum magnetic iron modified attapulgite phosphorus removal adsorbent; The mass ratio of the lanthanum salt, calcined attapulgite, divalent iron salt and trivalent iron salt is 1:(1.5~2.5):(0.5~1.5):(0.5~1.5); the lanthanum salt is at least one of lanthanum nitrate and lanthanum chloride; the divalent iron salt is one or more of ferrous sulfate heptahydrate, ferrous chloride, anhydrous ferrous sulfate or ferrous nitrate; the trivalent iron salt is one or more of ferric chloride, ferric sulfate or ferric nitrate; the particle size of the lanthanum magnetic iron modified attapulgite phosphorus removal adsorbent is ≤0.075mm.

2. The preparation method according to claim 1, characterized in that: The lanthanum chloride is lanthanum chloride hexahydrate.

3. The preparation method according to claim 1, characterized in that: The pH adjusting agent for adjusting the pH is one or more of sodium hydroxide, ammonia water, hydrochloric acid or sulfuric acid.

4. The preparation method according to claim 1, characterized in that: The heating temperature is 70-85°C.

5. The preparation method according to claim 1, characterized in that: The drying temperature is 60-75°C.

6. Use of the lanthanum magnetic iron modified attapulgite phosphorus removal adsorbent obtained by the preparation method of claim 1 in water bodies with a phosphorus concentration of ≤2 mg / L.