A waste-based mountain slope water-retaining and soil-solidifying material and its preparation method and application

By preparing waste-based water-retaining and solidifying materials for mountain slopes, the damage and grass planting of large slopes is solved by using the multiple crosslinking structures of kelp industrial wastewater, waste iron tailings powder, waste tea residue powder and bentonite. The problems of degradation and soil erosion have achieved ecological protection and efficient use of waste.

CN116375401BActive Publication Date: 2024-11-19CCCC LANDSCAPE SHANDONG CO +1
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202310352424.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-04
Publication Date
2024-11-19
Estimated Expiration
2043-04-04

AI Technical Summary

Technical Problem

The large slopes of the mountains have problems such as damage, serious grass degradation, and serious soil erosion. Poor waste treatment leads to environmental pollution, and lacks effective ecological protection measures.

Method used

Use waste-based mountain slope water-retaining and solidifying materials, including kelp industrial wastewater, waste iron tailings powder, waste tea residue powder, waste sweet potato residue and bentonite, and are prepared by grinding, stirring and mixing to form a multiple crosslinked colloid network. Structure, improves the water retention and curing properties of the material.

Benefits of technology

It realizes water retention and solidification of mountain slope soil, promotes vegetation growth, solves waste pollution problems, and has a simple process and low cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004162047340000111
    Figure BDA0004162047340000111
Patent Text Reader

Abstract

The present invention discloses a waste-based mountain slope water-retaining and soil-solidifying material, and a preparation method and application thereof, and belongs to the technical field of mountain slope water-retaining and soil-solidifying. The water-retaining and soil-solidifying material of the present invention comprises the following raw materials in parts by weight: 30 to 40 parts of kelp industrial wastewater, 10 to 15 parts of waste iron tailings powder, 15 to 30 parts of waste tea residue powder, 15 to 30 parts of waste sweet potato residue and 15 to 30 parts of bentonite; the preparation method is to mix the waste iron tailings powder with kelp industrial wastewater to obtain material A; mix the waste tea residue powder, waste sweet potato residue and kelp industrial wastewater to obtain material B; mix material A, material B and bentonite to obtain the water-retaining and soil-solidifying material. The water-retaining and soil-solidifying material of the present invention has good water-retaining and soil-solidifying properties for mountain slope soil, is beneficial to the solidification of mountain slope soil and improves its water-retaining properties, and is beneficial to the growth and development of mountain slope preparation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of mountain slope water-retaining and soil-solidifying technology, and in particular relates to a waste-based mountain slope water-retaining and soil-solidifying material, and a preparation method and application thereof. Background Art

[0002] The following problems often exist in steep mountains: (1) The damaged area of ​​the mountain is large and the cost of repair is high. Due to long-term mining, large areas of cliffs, rocks and soil with damaged physical structures have been formed. (2) The grass on the damaged mountain has seriously degraded and the vegetation type is single. Due to the poor supply of nutrients and water on the mountain slopes, the vegetation faces threats such as drought and heat and is extremely difficult to recover. (3) The slopes are covered with thin soil and the degree of soil erosion is serious. Due to long-term mountain excavation, the rock layer on the rock slope is thick, the overall slope is high and steep, and the nutrients in the soil are gradually lost over time, resulting in a decrease in fertility year by year, and the mountain slopes are short of water and soil.

[0003] At present, there are a lot of wastes in industrial, mining and agricultural production, including production wastewater, waste slag or plant scraps. The discharge or stacking of wastewater and waste slag will pollute the environment; the treatment of wastewater and waste slag will further consume energy and resources. Therefore, it is an urgent need for waste disposal in various industries to treat these wastes reasonably and efficiently and make full use of the useful components in them.

[0004] Therefore, if waste is used to solve the problem of steep mountains, it can not only make full use of the waste, but also provide ecological protection for the mountain slopes. Summary of the invention

[0005] In order to solve the above problems in the prior art, the present invention provides a waste-based mountain slope water-retaining and soil-fixing material, and a preparation method and application thereof.

[0006] To achieve the above object, the present invention provides the following technical solutions:

[0007] One of the technical solutions of the present invention: a waste-based mountain slope water-retaining and soil-solidifying material, which includes the following raw materials by weight: 30 to 40 parts of kelp industrial wastewater, 10 to 15 parts of waste iron tailings powder, 15 to 30 parts of waste tea residue powder, 15 to 30 parts of waste sweet potato residue and 15 to 30 parts of bentonite.

[0008] Furthermore, the preparation method of the waste iron tailings powder is: grinding the waste iron tailings powder to a fineness of 600 to 800 meshes.

[0009] Furthermore, the preparation method of the waste tea residue powder is: stirring and crushing the waste tea residue to a particle size of 100 to 200 meshes.

[0010] Furthermore, the preparation method of the waste sweet potato residue is: stirring and crushing the waste sweet potato residue to a particle size of 100 to 200 meshes.

[0011] Technical solution 2 of the present invention: The method for preparing the above-mentioned waste-based mountain slope water-retaining and soil-fixing material comprises the following steps:

[0012] 1) Mixing the waste iron tailings with part of the kelp industrial wastewater to obtain material A;

[0013] 2) Mixing the waste tea residue powder, waste sweet potato residue and remaining kelp industrial wastewater to obtain material B;

[0014] 3) Mixing the material A obtained in step 1), the material B obtained in step 2) and bentonite to obtain the waste-based mountain slope water-retaining and soil-solidifying material.

[0015] Furthermore, the weight ratio of part of the kelp industrial wastewater in step 1) to the remaining kelp industrial wastewater in step 2) is (0.5-1.5):(2-3).

[0016] Furthermore, the mixing in step 1) is carried out at 20-40° C. and a stirring speed of 600 r / min for 1 hour, followed by standing for 5 hours.

[0017] Furthermore, the mixing in step 2) is carried out at 20-40° C. and a stirring speed of 600 r / min for 1 hour, followed by standing for 3 hours.

[0018] Furthermore, the mixing in step 3) is carried out at 20-40° C. and a stirring speed of 800 r / min for 1 hour, followed by standing for 3 hours.

[0019] The third technical solution of the present invention: Application of the above waste-based mountain slope water-retaining and soil-consolidating material in mountain slope water-retaining and soil-consolidating.

[0020] Compared with the prior art, the present invention has the following beneficial effects:

[0021] The waste-based mountain slope water-retaining and soil-solidifying material of the present invention has good water-retaining performance and soil-solidifying performance, is beneficial to the solidification of mountain slope soil and improves its water-retaining performance, and is beneficial to the growth and development of mountain slope vegetation.

[0022] The waste-based mountain slope water-retaining and soil-solidifying material of the present invention makes full use of wastes from industrial, mining and agricultural production for processing, has a simple process and low cost, can not only solve the problem of waste pollution to the environment, but also solve the problem of soil water retention and solidification on the mountain slope.

[0023] Kelp industrial wastewater contains organic molecules such as sodium alginate, polysaccharides, cellulose and protein, as well as formaldehyde and calcium ions; waste iron tailings contain a large amount of iron oxides; waste tea residues and waste sweet potato residues contain a large amount of plant polyphenols, proteins, cellulose and pectin. These substances in the waste can build a multi-cross-linked colloidal network structure with bentonite, which can firmly adhere to the soil and rocks on the mountain slope and has excellent water retention performance.

[0024] Bentonite, waste tea residue powder and waste iron tailings powder provide an internal porous structure for the mountain slope water-retaining and soil-solidifying material of the present invention, thereby improving the water-retaining performance of the material; the slow release of iron ions in the iron tailings powder and polyphenols and proteins in the tea residue powder ensures the structural stability and adhesion of the material. DETAILED DESCRIPTION

[0025] Now, various exemplary embodiments of the present invention are described in detail, and this detailed description should not be considered as a limitation of the present invention, but should be understood as a more detailed description of certain aspects, characteristics and embodiments of the present invention. It should be understood that the terms described in the present invention are only for describing specific embodiments and are not used to limit the present invention.

[0026] In addition, for the numerical range in the present invention, it is understood that each intermediate value between the upper and lower limits of the range is also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.

[0027] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.

[0028] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to those skilled in the art. The present invention description and examples are exemplary only.

[0029] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.

[0030] Unless otherwise specified, the "parts" described in the present invention are all based on parts by weight.

[0031] In the following embodiments, the waste-based mountain slope water-retaining and soil-solidifying materials include the following raw materials, by weight: 30 to 40 parts of kelp industrial wastewater, 10 to 15 parts of waste iron tailings powder, 15 to 30 parts of waste tea residue powder, 15 to 30 parts of waste sweet potato residue and 15 to 30 parts of bentonite.

[0032] In some embodiments, the preparation method of the waste iron tailings powder is: grinding the waste iron tailings powder to a fineness of 600 to 800 meshes.

[0033] In some embodiments, the preparation method of the waste tea residue powder is: stirring and crushing the waste tea residue to a particle size of 100 to 200 meshes.

[0034] In some embodiments, the preparation method of the waste sweet potato residue is: stirring and crushing the waste sweet potato residue to a particle size of 100 to 200 meshes.

[0035] In some embodiments, a method for preparing a waste-based mountain slope water-retaining and soil-fixing material comprises the following steps:

[0036] 1) Mixing the waste iron tailings with part of the kelp industrial wastewater to obtain material A;

[0037] 2) Mixing the waste tea residue powder, waste sweet potato residue and remaining kelp industrial wastewater to obtain material B;

[0038] 3) Mixing the material A obtained in step 1), the material B obtained in step 2) and bentonite to obtain the waste-based mountain slope water-retaining and soil-solidifying material.

[0039] The weight ratio of the partial kelp industrial wastewater in step 1) to the remaining kelp industrial wastewater in step 2) is (0.5-1.5): (2-3)

[0040] The mixing in step 1) is performed at 20-40° C. and a stirring speed of 600 r / min for 1 hour, and then allowed to stand for 5 hours.

[0041] The mixing in step 2) is performed at 20-40° C. and a stirring speed of 600 r / min for 1 hour, and then allowed to stand for 3 hours.

[0042] The mixing in step 3) is performed at 20-40° C. and a stirring speed of 800 r / min for 1 hour, and then allowed to stand for 3 hours.

[0043] Example 1

[0044] 1) 10 parts of waste iron tailings powder (fineness of 600 mesh, particle size of 23 microns) were added to 10 parts of kelp industrial wastewater, mixed and stirred at a temperature of 40° C. and a stirring speed of 600 r / min for 1 hour, and then allowed to stand for 5 hours to obtain material A;

[0045] 2) adding 20 parts of waste tea residue powder (particle size of 150 microns) and 15 parts of waste sweet potato residue (particle size of 150 microns) to 30 parts of kelp industrial wastewater, mixing and stirring at a temperature of 40° C. and a stirring speed of 600 r / min for 1 hour, and then standing for 3 hours to obtain material B;

[0046] 3) Material A obtained in step 1), material B obtained in step 2) and 15 parts of bentonite were mixed, and the mixture was stirred at a temperature of 25° C. and a stirring speed of 800 r / min for 1 hour, and then allowed to stand for 3 hours to obtain a mountain slope water-retaining and soil-solidifying material.

[0047] Example 2

[0048] 1) 15 parts of waste iron tailings powder (fineness of 600 mesh, particle size of 23 microns) were added to 10 parts of kelp industrial wastewater, mixed and stirred at a temperature of 40° C. and a stirring speed of 600 r / min for 1 hour, and then allowed to stand for 5 hours to obtain material A;

[0049] 2) 15 parts of waste tea residue powder (particle size of 120 microns) and 15 parts of waste sweet potato residue (particle size of 150 microns) were added to 30 parts of kelp industrial wastewater, mixed and stirred at a temperature of 30° C. and a stirring speed of 600 r / min for 1 hour, and then allowed to stand for 3 hours to obtain material B;

[0050] 3) Material A obtained in step 1), material B obtained in step 2) and 15 parts of bentonite were mixed, and the mixture was stirred at a temperature of 25° C. and a stirring speed of 800 r / min for 1 hour, and then allowed to stand for 3 hours to obtain a mountain slope water-retaining and soil-solidifying material.

[0051] Example 3

[0052] 1) 10 parts of waste iron tailings powder (fineness of 800 mesh, particle size of 18 microns) were added to 10 parts of kelp industrial wastewater, mixed and stirred at a temperature of 20° C. and a stirring speed of 600 r / min for 1 hour, and then allowed to stand for 5 hours to obtain material A;

[0053] 2) 20 parts of waste tea residue powder (particle size of 120 microns) and 15 parts of waste sweet potato residue (particle size of 120 microns) were added to 25 parts of kelp industrial wastewater, mixed and stirred at a temperature of 40° C. and a stirring speed of 600 r / min for 1 hour, and then allowed to stand for 3 hours to obtain material B;

[0054] 3) Material A obtained in step 1), material B obtained in step 2) and 20 parts of bentonite are mixed, mixed and stirred at a temperature of 20° C. and a stirring speed of 800 r / min for 1 hour, and then allowed to stand for 3 hours to obtain a mountain slope water-retaining and soil-solidifying material.

[0055] Example 4

[0056] 1) 10 parts of waste iron tailings powder (fineness of 800 mesh, particle size of 18 microns) were added to 15 parts of kelp industrial wastewater, mixed and stirred at a temperature of 30° C. and a stirring speed of 600 r / min for 1 hour, and then allowed to stand for 5 hours to obtain material A;

[0057] 2) adding 20 parts of waste tea residue powder (particle size of 106 microns) and 20 parts of waste sweet potato residue (particle size of 150 microns) to 20 parts of kelp industrial wastewater, mixing and stirring at a temperature of 25° C. and a stirring speed of 600 r / min for 1 hour, and then standing for 3 hours to obtain material B;

[0058] 3) Material A obtained in step 1), material B obtained in step 2) and 15 parts of bentonite were mixed, and the mixture was stirred at a temperature of 30° C. and a stirring speed of 800 r / min for 1 hour, and then allowed to stand for 3 hours to obtain a mountain slope water-retaining and soil-solidifying material.

[0059] Example 5

[0060] 1) 10 parts of waste iron tailings powder (fineness of 800 mesh, particle size of 18 microns) were added to 10 parts of kelp industrial wastewater, mixed and stirred at a temperature of 35° C. and a stirring speed of 600 r / min for 1 hour, and then allowed to stand for 5 hours to obtain material A;

[0061] 2) 15 parts of waste tea residue powder (particle size of 75 microns) and 20 parts of waste sweet potato residue (particle size of 150 microns) were added to 25 parts of kelp industrial wastewater, mixed and stirred at a temperature of 20° C. and a stirring speed of 600 r / min for 1 hour, and then allowed to stand for 3 hours to obtain material B;

[0062] 3) Material A obtained in step 1), material B obtained in step 2) and 20 parts of bentonite are mixed, and the mixture is stirred at a temperature of 30° C. and a stirring speed of 800 r / min for 1 hour, and then allowed to stand for 3 hours to obtain a mountain slope water-retaining and soil-solidifying material.

[0063] Example 6

[0064] 1) 10 parts of waste iron tailings powder (fineness of 800 mesh, particle size of 18 microns) were added to 5 parts of kelp industrial wastewater, mixed and stirred at a temperature of 20° C. and a stirring speed of 600 r / min for 1 hour, and then allowed to stand for 5 hours to obtain material A;

[0065] 2) 15 parts of waste tea residue powder (particle size of 75 microns) and 30 parts of waste sweet potato residue (particle size of 106 microns) were added to 25 parts of kelp industrial wastewater, mixed and stirred at a temperature of 25° C. and a stirring speed of 600 r / min for 1 hour, and then allowed to stand for 3 hours to obtain material B;

[0066] 3) Material A obtained in step 1), material B obtained in step 2) and 15 parts of bentonite were mixed, and the mixture was stirred at a temperature of 30° C. and a stirring speed of 800 r / min for 1 hour, and then allowed to stand for 3 hours to obtain a mountain slope water-retaining and soil-solidifying material.

[0067] Comparative Example 1

[0068] Same as Example 1, the only difference is that seawater is used to replace kelp industrial wastewater in step 1) and step 2).

[0069] Comparative Example 2

[0070] 1) 20 parts of waste tea residue powder (particle size of 120 microns) and 15 parts of waste sweet potato residue (particle size of 150 microns) were added to 30 parts of kelp industrial wastewater, mixed and stirred at a temperature of 40° C. and a stirring speed of 600 r / min for 1 hour, and then allowed to stand for 3 hours to obtain material B;

[0071] 2) Material B obtained in step 1) was mixed with 15 parts of bentonite, and the mixture was stirred at a temperature of 25° C. and a stirring speed of 800 r / min for 1 hour, and then allowed to stand for 3 hours to obtain a mountain slope water-retaining and soil-solidifying material.

[0072] Comparative Example 3

[0073] The same as Example 1, except that the addition of waste tea residue powder in step 2) is omitted.

[0074] Comparative Example 4

[0075] The same as Example 1, except that the addition of waste sweet potato residue in step 2) is omitted.

[0076] Comparative Example 5

[0077] Same as Example 1, except that kaolin is used to replace bentonite in step 3).

[0078] Performance Testing

[0079] 1. Water retention performance

[0080] The water-retaining soil-solidifying materials for mountain slopes prepared in Examples 1 to 6 and Comparative Examples 1 to 5 were tested for their water-retaining performance. Important indicators for judging water-retaining performance: (1) Water absorption capacity, usually expressed as water absorption rate. Water absorption rate = the ratio (percentage) of the mass of water absorbed by the water-retaining material to its own mass. (2) Repeated water absorption capacity determination: At room temperature, the water-retaining material that has completely absorbed water is placed in a drying oven at 70°C to dry and dehydrate to constant weight, then cooled to room temperature, and then placed in distilled water in the same environment to absorb water. After 5 drying-water absorption cycles, the reusability of the water-retaining material is tested. Repeated drying water absorption rate = water absorption rate after drying / original water absorption rate. (3) Water retention capacity determination: The water-retaining material after water absorption is placed in a centrifuge with a rotation speed of 4000r / min, and after centrifugation for 1h, the water retention rate is determined. Water retention rate = mass of water-retaining material after centrifugation / mass of water-retaining material before centrifugation. All water used is deionized water.

[0081] The test results are shown in Table 1;

[0082] Table 1 Water retention performance

[0083] Water absorption (%) Repeated drying water absorption (%) Water retention rate (%) Example 1 212 92 96 Example 2 201 91 96 Example 3 203 89 95 Example 4 225 90 98 Example 5 234 93 97 Example 6 213 92 93 Comparative Example 1 110 67 90 Comparative Example 2 106 73 85 Comparative Example 3 104 63 80 Comparative Example 4 102 68 86 Comparative Example 5 107 71 92

[0084] 2. Soil solidification performance

[0085] The mountain slope water-retaining materials prepared in Examples 1 to 6 and Comparative Examples 1 to 5 were mixed with the local slope soil in Jinan to test the soil-fixing performance. The test method was as follows: the slope soil was crushed to 100 meshes and dried for later use. The mountain slope water-retaining and soil-fixing materials were mixed evenly with the slope soil in a ratio of 20:80, and an appropriate amount of water was added to adjust the optimum moisture content, and then placed in a test mold with a size of 40mm×40mm×40mm to prepare a molded sample. The molded test piece was wrapped and sealed with a plastic wrap, placed in an environment with a temperature of 20±1°C and a relative humidity of more than 92% for curing, and demolded after curing for 24 hours, and then the demolded test piece was further wrapped and sealed with a plastic wrap, and placed in an environment with a temperature of 20±1°C and a relative humidity of more than 92% for curing for 7 days. The water absorption rate, wet-dry strength, and water stability coefficient of the sample were tested to evaluate the curing performance of the water-retaining and soil-fixing material on the slope soil. The water stability coefficient = the unconfined compressive strength of the sample after 6 days of standard curing plus 24 hours of immersion / the unconfined compressive strength of the sample after 7 days of standard curing. The test results are shown in Table 2;

[0086] Table 2 Soil solidification performance

[0087]

[0088] The above description is only a preferred specific implementation manner of the present invention, and the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, and they should be covered by the protection scope of the present invention.

Claims

1. A waste-based mountain slope water-retaining and soil-solidifying material, characterized in that: The invention is composed of the following raw materials by weight: 30 to 40 parts of kelp industrial waste water, 10 to 15 parts of waste iron tailings powder, 15 to 30 parts of waste tea residue powder, 15 to 30 parts of waste sweet potato residue and 15 to 30 parts of bentonite; The preparation method of the waste iron tailings powder is as follows: grinding the waste iron tailings powder to a fineness of 600 to 800 meshes; The preparation method of the waste tea residue powder is as follows: stirring and crushing the waste tea residue to a particle size of 100 to 200 meshes; The preparation method of the waste sweet potato residue is as follows: the waste sweet potato residue is stirred and crushed to a particle size of 100 to 200 meshes.

2. A method for preparing the waste-based mountain slope water-retaining and soil-fixing material according to claim 1, characterized in that: The following steps are involved: 1) Mixing the waste iron tailings with part of the kelp industrial wastewater to obtain material A; 2) Mixing the waste tea residue powder, waste sweet potato residue and remaining kelp industrial wastewater to obtain material B; 3) Mixing the material A obtained in step 1), the material B obtained in step 2) and bentonite to obtain the waste-based mountain slope water-retaining and soil-solidifying material.

3. The preparation method according to claim 2, characterized in that: The weight ratio of part of the kelp industrial wastewater in step 1) to the remaining kelp industrial wastewater in step 2) is (0.5-1.5): (2-3).

4. The preparation method according to claim 2, characterized in that: The mixing in step 1) is performed at 20-40° C. and a stirring speed of 600 r / min for 1 hour, and then allowed to stand for 5 hours.

5. The preparation method according to claim 2, characterized in that: The mixing in step 2) is performed at 20-40° C. and a stirring speed of 600 r / min for 1 hour, and then allowed to stand for 3 hours.

6. The preparation method according to claim 2, characterized in that: The mixing in step 3) is performed at 20-40° C. and a stirring speed of 800 r / min for 1 hour, and then allowed to stand for 3 hours.

7. Use of the waste-based mountain slope water-retaining and soil-fixing material according to claim 1 in mountain slope water-retaining and soil-fixing.

Citation Information

Cited By

  • Nano-modified water-retention soil-fixation material and preparation method thereof

    CN121379599A